<?xml version="1.0"?>
<feed xmlns="http://www.w3.org/2005/Atom" xml:lang="en">
	<id>https://labadviser.nanolab.dtu.dk//index.php?action=history&amp;feed=atom&amp;title=Specific_Process_Knowledge%2FEtch%2FDRIE%2FPegasus-3%2FDREM%2FDREM_0.5kW_v2.3</id>
	<title>Specific Process Knowledge/Etch/DRIE/Pegasus-3/DREM/DREM 0.5kW v2.3 - Revision history</title>
	<link rel="self" type="application/atom+xml" href="https://labadviser.nanolab.dtu.dk//index.php?action=history&amp;feed=atom&amp;title=Specific_Process_Knowledge%2FEtch%2FDRIE%2FPegasus-3%2FDREM%2FDREM_0.5kW_v2.3"/>
	<link rel="alternate" type="text/html" href="https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Etch/DRIE/Pegasus-3/DREM/DREM_0.5kW_v2.3&amp;action=history"/>
	<updated>2026-08-27T13:32:47Z</updated>
	<subtitle>Revision history for this page on the wiki</subtitle>
	<generator>MediaWiki 1.43.3</generator>
	<entry>
		<id>https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Etch/DRIE/Pegasus-3/DREM/DREM_0.5kW_v2.3&amp;diff=51499&amp;oldid=prev</id>
		<title>Jmli at 06:33, 4 April 2025</title>
		<link rel="alternate" type="text/html" href="https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Etch/DRIE/Pegasus-3/DREM/DREM_0.5kW_v2.3&amp;diff=51499&amp;oldid=prev"/>
		<updated>2025-04-04T06:33:24Z</updated>

		<summary type="html">&lt;p&gt;&lt;/p&gt;
&lt;table style=&quot;background-color: #fff; color: #202122;&quot; data-mw=&quot;interface&quot;&gt;
				&lt;col class=&quot;diff-marker&quot; /&gt;
				&lt;col class=&quot;diff-content&quot; /&gt;
				&lt;col class=&quot;diff-marker&quot; /&gt;
				&lt;col class=&quot;diff-content&quot; /&gt;
				&lt;tr class=&quot;diff-title&quot; lang=&quot;en&quot;&gt;
				&lt;td colspan=&quot;2&quot; style=&quot;background-color: #fff; color: #202122; text-align: center;&quot;&gt;← Older revision&lt;/td&gt;
				&lt;td colspan=&quot;2&quot; style=&quot;background-color: #fff; color: #202122; text-align: center;&quot;&gt;Revision as of 08:33, 4 April 2025&lt;/td&gt;
				&lt;/tr&gt;&lt;tr&gt;&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot; id=&quot;mw-diff-left-l1&quot;&gt;Line 1:&lt;/td&gt;
&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot;&gt;Line 1:&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;−&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt; &lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;+&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;&lt;ins style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;&amp;lt;!--Checked for updates on 4/4-2025 - ok/jmli --&amp;gt;&lt;/ins&gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;/table&gt;</summary>
		<author><name>Jmli</name></author>
	</entry>
	<entry>
		<id>https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Etch/DRIE/Pegasus-3/DREM/DREM_0.5kW_v2.3&amp;diff=39830&amp;oldid=prev</id>
		<title>Jmli: Blanked the page</title>
		<link rel="alternate" type="text/html" href="https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Etch/DRIE/Pegasus-3/DREM/DREM_0.5kW_v2.3&amp;diff=39830&amp;oldid=prev"/>
		<updated>2022-01-21T09:28:33Z</updated>

		<summary type="html">&lt;p&gt;Blanked the page&lt;/p&gt;
&lt;a href=&quot;https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Etch/DRIE/Pegasus-3/DREM/DREM_0.5kW_v2.3&amp;amp;diff=39830&amp;amp;oldid=39546&quot;&gt;Show changes&lt;/a&gt;</summary>
		<author><name>Jmli</name></author>
	</entry>
	<entry>
		<id>https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Etch/DRIE/Pegasus-3/DREM/DREM_0.5kW_v2.3&amp;diff=39546&amp;oldid=prev</id>
		<title>Jmli at 14:25, 2 December 2021</title>
		<link rel="alternate" type="text/html" href="https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Etch/DRIE/Pegasus-3/DREM/DREM_0.5kW_v2.3&amp;diff=39546&amp;oldid=prev"/>
		<updated>2021-12-02T14:25:47Z</updated>

		<summary type="html">&lt;p&gt;&lt;/p&gt;
&lt;table style=&quot;background-color: #fff; color: #202122;&quot; data-mw=&quot;interface&quot;&gt;
				&lt;col class=&quot;diff-marker&quot; /&gt;
				&lt;col class=&quot;diff-content&quot; /&gt;
				&lt;col class=&quot;diff-marker&quot; /&gt;
				&lt;col class=&quot;diff-content&quot; /&gt;
				&lt;tr class=&quot;diff-title&quot; lang=&quot;en&quot;&gt;
				&lt;td colspan=&quot;2&quot; style=&quot;background-color: #fff; color: #202122; text-align: center;&quot;&gt;← Older revision&lt;/td&gt;
				&lt;td colspan=&quot;2&quot; style=&quot;background-color: #fff; color: #202122; text-align: center;&quot;&gt;Revision as of 16:25, 2 December 2021&lt;/td&gt;
				&lt;/tr&gt;&lt;tr&gt;&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot; id=&quot;mw-diff-left-l57&quot;&gt;Line 57:&lt;/td&gt;
&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot;&gt;Line 57:&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;|-  &lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;|-  &lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;|16/6-2021&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;|16/6-2021&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;−&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;|&lt;del style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;Morten Foss &lt;/del&gt;wafer&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;+&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;|&lt;ins style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;150 mm &lt;/ins&gt;wafer &lt;ins style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;with standard DUV resist and a pattern of pillars of variable densities/widths&lt;/ins&gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;|Si /  10%&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;|Si /  10%&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;|C06695.14&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;|C06695.14&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;/table&gt;</summary>
		<author><name>Jmli</name></author>
	</entry>
	<entry>
		<id>https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Etch/DRIE/Pegasus-3/DREM/DREM_0.5kW_v2.3&amp;diff=39545&amp;oldid=prev</id>
		<title>Jmli at 14:23, 2 December 2021</title>
		<link rel="alternate" type="text/html" href="https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Etch/DRIE/Pegasus-3/DREM/DREM_0.5kW_v2.3&amp;diff=39545&amp;oldid=prev"/>
		<updated>2021-12-02T14:23:11Z</updated>

		<summary type="html">&lt;p&gt;&lt;/p&gt;
&lt;table style=&quot;background-color: #fff; color: #202122;&quot; data-mw=&quot;interface&quot;&gt;
				&lt;col class=&quot;diff-marker&quot; /&gt;
				&lt;col class=&quot;diff-content&quot; /&gt;
				&lt;col class=&quot;diff-marker&quot; /&gt;
				&lt;col class=&quot;diff-content&quot; /&gt;
				&lt;tr class=&quot;diff-title&quot; lang=&quot;en&quot;&gt;
				&lt;td colspan=&quot;2&quot; style=&quot;background-color: #fff; color: #202122; text-align: center;&quot;&gt;← Older revision&lt;/td&gt;
				&lt;td colspan=&quot;2&quot; style=&quot;background-color: #fff; color: #202122; text-align: center;&quot;&gt;Revision as of 16:23, 2 December 2021&lt;/td&gt;
				&lt;/tr&gt;&lt;tr&gt;&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot; id=&quot;mw-diff-left-l17&quot;&gt;Line 17:&lt;/td&gt;
&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot;&gt;Line 17:&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;|-&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;|-&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;|16/6-2021&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;|16/6-2021&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;−&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;|PegReticle &lt;del style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;wafer&lt;/del&gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;+&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;|&lt;ins style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;150 mm wafer with standard DUV resist and &lt;/ins&gt;PegReticle &lt;ins style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;pattern&lt;/ins&gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;|Si /  25-50%&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;|Si /  25-50%&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;|C06692.03 pegreticle wafer&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;|C06692.03 pegreticle wafer&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;/table&gt;</summary>
		<author><name>Jmli</name></author>
	</entry>
	<entry>
		<id>https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Etch/DRIE/Pegasus-3/DREM/DREM_0.5kW_v2.3&amp;diff=39544&amp;oldid=prev</id>
		<title>Jmli: Created page with &quot;{| border=&quot;2&quot; cellpadding=&quot;0&quot; cellspacing=&quot;0&quot; style=&quot;text-align:center;&quot; |- ! rowspan=&quot;2&quot; width=&quot;40&quot;| Date ! colspan=&quot;2&quot; width=&quot;120&quot;| Substrate Information ! colspan=&quot;4&quot; | Pro...&quot;</title>
		<link rel="alternate" type="text/html" href="https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Etch/DRIE/Pegasus-3/DREM/DREM_0.5kW_v2.3&amp;diff=39544&amp;oldid=prev"/>
		<updated>2021-12-02T14:21:48Z</updated>

		<summary type="html">&lt;p&gt;Created page with &amp;quot;{| border=&amp;quot;2&amp;quot; cellpadding=&amp;quot;0&amp;quot; cellspacing=&amp;quot;0&amp;quot; style=&amp;quot;text-align:center;&amp;quot; |- ! rowspan=&amp;quot;2&amp;quot; width=&amp;quot;40&amp;quot;| Date ! colspan=&amp;quot;2&amp;quot; width=&amp;quot;120&amp;quot;| Substrate Information ! colspan=&amp;quot;4&amp;quot; | Pro...&amp;quot;&lt;/p&gt;
&lt;p&gt;&lt;b&gt;New page&lt;/b&gt;&lt;/p&gt;&lt;div&gt;{| border=&amp;quot;2&amp;quot; cellpadding=&amp;quot;0&amp;quot; cellspacing=&amp;quot;0&amp;quot; style=&amp;quot;text-align:center;&amp;quot;&lt;br /&gt;
|-&lt;br /&gt;
! rowspan=&amp;quot;2&amp;quot; width=&amp;quot;40&amp;quot;| Date&lt;br /&gt;
! colspan=&amp;quot;2&amp;quot; width=&amp;quot;120&amp;quot;| Substrate Information&lt;br /&gt;
! colspan=&amp;quot;4&amp;quot; | Process Information&lt;br /&gt;
! colspan=&amp;quot;3&amp;quot; width=&amp;quot;200&amp;quot; | Results&lt;br /&gt;
|-&lt;br /&gt;
! width=&amp;quot;30&amp;quot; | Wafer info&lt;br /&gt;
! width=&amp;quot;40&amp;quot; | Material/ Exposed area&lt;br /&gt;
! width=&amp;quot;40&amp;quot; | Condi- tioning&lt;br /&gt;
! width=&amp;quot;40&amp;quot; | Recipe&lt;br /&gt;
! width=&amp;quot;40&amp;quot; | Wafer ID&lt;br /&gt;
! width=&amp;quot;40&amp;quot; | Comments&lt;br /&gt;
! width=&amp;quot;400&amp;quot; |SEM images&lt;br /&gt;
! width=&amp;quot;100&amp;quot; |Picoscope &lt;br /&gt;
! width=&amp;quot;600&amp;quot; |Numbers &lt;br /&gt;
|-&lt;br /&gt;
|16/6-2021&lt;br /&gt;
|PegReticle wafer&lt;br /&gt;
|Si /  25-50%&lt;br /&gt;
|C06692.03 pegreticle wafer&lt;br /&gt;
|nanolab/ jmli / DREM / DREM 0.5kW v2.3, 50 cycles or 4:35 minutes&lt;br /&gt;
|C06694.01&lt;br /&gt;
|[http://labmanager.dtu.dk/function.php?module=Processlog&amp;amp;view=editlog&amp;amp;usageid=388881 Process log entry]&lt;br /&gt;
| &lt;br /&gt;
[[file:C06694.01c153.png |120px|frameless ]]&lt;br /&gt;
[[file:C06694.01c154.png |120px|frameless ]]&lt;br /&gt;
[[file:C06694.01c155.png |120px|frameless ]]&lt;br /&gt;
[[file:C06694.01c156.png |120px|frameless ]]&lt;br /&gt;
[[file:C06694.01c157.png |120px|frameless ]]&lt;br /&gt;
[[file:C06694.01c158.png |120px|frameless ]]&lt;br /&gt;
| &amp;lt;!-- Add picos here:[[file:S014009 1.gif |120px|frameless ]] --&amp;gt;&lt;br /&gt;
| &lt;br /&gt;
{| {{table}} &lt;br /&gt;
| align=&amp;quot;center&amp;quot; style=&amp;quot;background:#f0f0f0;&amp;quot;|&amp;#039;&amp;#039;&amp;#039;SEM image:&amp;#039;&amp;#039;&amp;#039;&lt;br /&gt;
| align=&amp;quot;center&amp;quot; style=&amp;quot;background:#f0f0f0;&amp;quot;|&amp;#039;&amp;#039;&amp;#039;[http://labadviser.nanolab.dtu.dk/index.php/File:C06694.01c155.png c155]&amp;#039;&amp;#039;&amp;#039;&lt;br /&gt;
| align=&amp;quot;center&amp;quot; style=&amp;quot;background:#f0f0f0;&amp;quot;|&amp;#039;&amp;#039;&amp;#039;[http://labadviser.nanolab.dtu.dk/index.php/File:C06694.01c157.png c157]&amp;#039;&amp;#039;&amp;#039;&lt;br /&gt;
| align=&amp;quot;center&amp;quot; style=&amp;quot;background:#f0f0f0;&amp;quot;|&amp;#039;&amp;#039;&amp;#039;[http://labadviser.nanolab.dtu.dk/index.php/File:C06694.01c153.png c153]&amp;#039;&amp;#039;&amp;#039;&lt;br /&gt;
|- &lt;br /&gt;
| Trench width (um)||0.21||0.79||0.84&lt;br /&gt;
|- &lt;br /&gt;
| Etched depth (um)||1.08||1.27||1.41&lt;br /&gt;
|- &lt;br /&gt;
| Etch rate (um/min)||0.24||0.28||0.31&lt;br /&gt;
|- &lt;br /&gt;
| &amp;lt;span title=&amp;quot;The cycles will vary if the aspect ratio is large &amp;quot;&amp;gt; Etch rate (nm/cyc) &amp;lt;/span&amp;gt;||21.61||25.46||28.14&lt;br /&gt;
|- &lt;br /&gt;
| Sidewall bowing (%)||0||1||0&lt;br /&gt;
|- &lt;br /&gt;
| Sidewall angle (degs)||90.31||90.19||90.3&lt;br /&gt;
|- &lt;br /&gt;
| Bottom bowing (%)||40.66||22.98||21.46&lt;br /&gt;
|- &lt;br /&gt;
|Aspect ratio||5.04||1.6||1.67&lt;br /&gt;
|- &lt;br /&gt;
|}&lt;br /&gt;
|- &lt;br /&gt;
|16/6-2021&lt;br /&gt;
|Morten Foss wafer&lt;br /&gt;
|Si /  10%&lt;br /&gt;
|C06695.14&lt;br /&gt;
|nanolab/ vy / DREM / DREM 0.5 kW v2.3 75 cyc or 6:52.5 mins&lt;br /&gt;
|C06694.01&lt;br /&gt;
|[http://labmanager.dtu.dk/function.php?module=Processlog&amp;amp;view=editlog&amp;amp;usageid=388881 Process log entry]&lt;br /&gt;
| &lt;br /&gt;
[[file:C06695.14c159.png |120px|frameless ]]&lt;br /&gt;
[[file:C06695.14c160.png |120px|frameless ]]&lt;br /&gt;
[[file:C06695.14c161.png |120px|frameless ]]&lt;br /&gt;
[[file:C06695.14c162.png |120px|frameless ]]&lt;br /&gt;
[[file:C06695.14c163.png |120px|frameless ]]&lt;br /&gt;
| &amp;lt;!-- Add picoscope links here:[[file:C06694.14 |120px|frameless ]] --&amp;gt;&lt;br /&gt;
| &lt;br /&gt;
{| {{table}} &lt;br /&gt;
| align=&amp;quot;center&amp;quot; style=&amp;quot;background:#f0f0f0;&amp;quot;|&amp;#039;&amp;#039;&amp;#039;SEM image:&amp;#039;&amp;#039;&amp;#039;&lt;br /&gt;
|- &lt;br /&gt;
| Trench width (um)&lt;br /&gt;
|- &lt;br /&gt;
| Etched depth (um)&lt;br /&gt;
|- &lt;br /&gt;
| Etch rate (um/min)&lt;br /&gt;
|- &lt;br /&gt;
| &amp;lt;span title=&amp;quot;The cycles will vary if the aspect ratio is large &amp;quot;&amp;gt; Etch rate (nm/cyc) &amp;lt;/span&amp;gt;&lt;br /&gt;
|- &lt;br /&gt;
| Sidewall bowing (%)&lt;br /&gt;
|- &lt;br /&gt;
| Sidewall angle (degs)&lt;br /&gt;
|- &lt;br /&gt;
| Bottom bowing (%)&lt;br /&gt;
|- &lt;br /&gt;
|Aspect ratio&lt;br /&gt;
|- &lt;br /&gt;
|}&lt;br /&gt;
|-&lt;br /&gt;
|27/9-2021&lt;br /&gt;
|DUV litho wafer,&lt;br /&gt;
|Si /  25-50%&lt;br /&gt;
|C06873.01&lt;br /&gt;
|nanolab/ jmli / DREM / DREM 0.5kW peg3, 100 cycles or 9:10 minutes&lt;br /&gt;
|C06873.02&lt;br /&gt;
|30 sec O2 0.2kW barc[http://labmanager.dtu.dk/function.php?module=Processlog&amp;amp;view=editlog&amp;amp;usageid=397212 Process log entry]&lt;br /&gt;
| &lt;br /&gt;
[[file:C06873.02c156.png |120px|frameless ]]&lt;br /&gt;
[[file:C06873.02c157.png |120px|frameless ]]&lt;br /&gt;
[[file:C06873.02c158.png |120px|frameless ]]&lt;br /&gt;
[[file:C06873.02c159.png |120px|frameless ]]&lt;br /&gt;
[[file:C06873.02c160.png |120px|frameless ]]&lt;br /&gt;
[[file:C06873.02c161.png |120px|frameless ]]&lt;br /&gt;
[[file:C06873.02c162.png |120px|frameless ]]&lt;br /&gt;
[[file:C06873.02c163.png |120px|frameless ]]&lt;br /&gt;
| &amp;lt;!-- Add picoscope links here:[[file:C06873.02 |120px|frameless ]] --&amp;gt;&lt;br /&gt;
| &lt;br /&gt;
{| {{table}} &lt;br /&gt;
| align=&amp;quot;center&amp;quot; style=&amp;quot;background:#f0f0f0;&amp;quot;|&amp;#039;&amp;#039;&amp;#039;SEM image:&amp;#039;&amp;#039;&amp;#039;&lt;br /&gt;
| align=&amp;quot;center&amp;quot; style=&amp;quot;background:#f0f0f0;&amp;quot;|&amp;#039;&amp;#039;&amp;#039;[http://labadviser.nanolab.dtu.dk/index.php/File:C06873.02c157.png c157]&amp;#039;&amp;#039;&amp;#039;&lt;br /&gt;
| align=&amp;quot;center&amp;quot; style=&amp;quot;background:#f0f0f0;&amp;quot;|&amp;#039;&amp;#039;&amp;#039;[http://labadviser.nanolab.dtu.dk/index.php/File:C06873.02c158.png c158]&amp;#039;&amp;#039;&amp;#039;&lt;br /&gt;
| align=&amp;quot;center&amp;quot; style=&amp;quot;background:#f0f0f0;&amp;quot;|&amp;#039;&amp;#039;&amp;#039;[http://labadviser.nanolab.dtu.dk/index.php/File:C06873.02c159.png c159]&amp;#039;&amp;#039;&amp;#039;&lt;br /&gt;
| align=&amp;quot;center&amp;quot; style=&amp;quot;background:#f0f0f0;&amp;quot;|&amp;#039;&amp;#039;&amp;#039;[http://labadviser.nanolab.dtu.dk/index.php/File:C06873.02c161.png c161]&amp;#039;&amp;#039;&amp;#039;&lt;br /&gt;
| align=&amp;quot;center&amp;quot; style=&amp;quot;background:#f0f0f0;&amp;quot;|&amp;#039;&amp;#039;&amp;#039;[http://labadviser.nanolab.dtu.dk/index.php/File:C06873.02c162.png c162]&amp;#039;&amp;#039;&amp;#039;&lt;br /&gt;
| align=&amp;quot;center&amp;quot; style=&amp;quot;background:#f0f0f0;&amp;quot;|&amp;#039;&amp;#039;&amp;#039;[http://labadviser.nanolab.dtu.dk/index.php/File:C06873.02c160.png c160]&amp;#039;&amp;#039;&amp;#039;&lt;br /&gt;
| align=&amp;quot;center&amp;quot; style=&amp;quot;background:#f0f0f0;&amp;quot;|&amp;#039;&amp;#039;&amp;#039;[http://labadviser.nanolab.dtu.dk/index.php/File:C06873.02c156.png c156]&amp;#039;&amp;#039;&amp;#039;&lt;br /&gt;
| align=&amp;quot;center&amp;quot; style=&amp;quot;background:#f0f0f0;&amp;quot;|&amp;#039;&amp;#039;&amp;#039;[http://labadviser.nanolab.dtu.dk/index.php/File:C06873.02c163.png c163]&amp;#039;&amp;#039;&amp;#039;&lt;br /&gt;
|- &lt;br /&gt;
| Trench width (um)||0.17||0.22||0.25||0.42||0.43||0.52||0.55||2.03&lt;br /&gt;
|- &lt;br /&gt;
| Etched depth (um)||1.3||1.36||1.4||1.56||1.57||1.62||1.64||1.87&lt;br /&gt;
|- &lt;br /&gt;
| Etch rate (um/min)||0.14||0.15||0.15||0.17||0.17||0.18||0.18||0.2&lt;br /&gt;
|- &lt;br /&gt;
| &amp;lt;span title=&amp;quot;The cycles will vary if the aspect ratio is large &amp;quot;&amp;gt; Etch rate (nm/cyc) &amp;lt;/span&amp;gt;||13||14||14||16||16||16||16||19&lt;br /&gt;
|- &lt;br /&gt;
| Sidewall bowing (%)||0||0.2||0.2||0.3||0.4||0.1||-0.1||0.1&lt;br /&gt;
|- &lt;br /&gt;
| Sidewall angle (degs)||89.38||89.33||89.41||89.29||89.43||89.44||89.4||89.21&lt;br /&gt;
|- &lt;br /&gt;
| Bottom bowing (%)||34.34||24.69||27.76||23.55||22.1||20.81||23.56||11.77&lt;br /&gt;
|- &lt;br /&gt;
|Aspect ratio||8.11||6.63||5.94||3.85||3.77||3.22||3.1||0.93&lt;br /&gt;
|- &lt;br /&gt;
|}&lt;br /&gt;
|- &lt;br /&gt;
|}&lt;/div&gt;</summary>
		<author><name>Jmli</name></author>
	</entry>
</feed>