Specific Process Knowledge/Bonding
Jump to navigation
Jump to search
Choose bonding method
- Eutectic bonding
- Fusion bonding
- Anodic bonding
Comparing the three bonding methods in the EVG NIL
. | Eutectic bonding | Fusion bonding | Anodic bonding |
---|---|---|---|
General description | For bonding two substrates by use of an interphase that makes an eutecticum. | For bonding two identical materials. | For bonding Si and Glass. |
Bonding temperature | Depending on the eutecticum 310C to 400C. | Depending on defects 50C to 400C. | Depending on the voltage 300C to 500C Standard is 400C. |
Annnealing temperature | No annealing | 1000C in the bond furnace C3 | No annealing |
Materials possible to bond | Bonding of substrates is done by use of the eutectica Au/Si, Au/Sn and Ni/Si | Si/Si, SiO/SiO | Si/Pyrex (glass) |
Substrate size | Up to 6" | Up to 6" | Up to 6" |
Cleaning | Cleaning by N2. | Wet chemical cleaning, IMEC. | Cleaning by N2. |
Choose equipment
- Speedline manual spinner - For spinning of PMMA and Topas
- EVG
- EVG NIL