Specific Process Knowledge/Thin film deposition/Furnace LPCVD Nitride

From LabAdviser

At the moment we have one LPCVD furnace for nitride depositions.

A few words about the furnace

The furnace is a Tempress horisontal furnace. The process is a batch process meaning you can run a batch of 25 wafers at a time. The deposition takes place at temperatures of 800-835 degrees Celsius. The reactive gases are Ammonia and dichlorsilane. The LPCVD nitride has a good step coverage and the film thickness is very uniform over the wafer. We have two standard LPCVD nitride processes: One for depositing stoichiometric nitride (Si3N4) and one for deposition of low stress nitride (SNR).


LPCVD
Stoichiometry
  • Si3N4
  • SRN

SRN: Silicon Rich Nitride

Film thickness
  • Si3N4:~50Å - ~3000Å
  • SRN: ~50Å - ~10000Å
Process Temperature
  • 800-835 oC
Step coverage
  • Good
Film quality
  • Dense film
  • Few defects
Batch size
  • 1-25 4" wafer per run
  • deposition on both sides of the substrate
Substrate material allowed
  • Silicon wafers
    • with layers of silicon oxide or silicon (oxy)nitride
  • Quartz wafers

Process Knowledge

Please take a look at the process side for deposition of Silicon Nitride using LPCVD: Deposition of Silicon Nitride using LPCVD