Specific Process Knowledge/Etch/AOE (Advanced Oxide Etch)/Remove resist in the AOE
- Feedback to this page: click here
Unless otherwise stated, this page is written by DTU Nanolab internal
Remove AZ resist in the AOE using the recipe Descum
Parameter | Descum (also settings for TDESC10M 20241029) |
---|---|
Coil Power [W] | 2000 |
Platen Power [W] | 30 |
Platen temperature [oC] | 0 |
O flow [sccm] | 99 |
Pressure [mTorr] | 10.0 (strike pressure 20.0 mTorr) |
Typical results | tested by bge@nanolab |
---|---|
AZ resist etch rate | ~41 nm/s |
BARC etching
I have tried once etching BARC with recipe SiO2_res:
Parameter | Recipe: SiO2_res | Recipe: Barcetch |
---|---|---|
Coil Power [W] | 1300 | 400 |
Platen Power [W] | 200 | 100 |
Platen temperature [oC] | 0 | 0 |
He flow [sccm] | 174 | 0 |
CF flow [sccm] | 5 | 0 |
CF4 flow [sccm] | 0 | 4 |
H flow [sccm] | 4 | 20 |
Pressure [mTorr] | 4 | 1 |
Etch rate in BARC [nm/sec] | 2 | 1 |
Selectivity to DUV resist [Barc:resist] | ? | [1-2:1] |