Specific Process Knowledge/Characterization/XRD/XRD SmartLab/Instrumental broading in GiXRD
This page describes values of Instrumental broadening in GiXRD measurements, and can be used as a reference for peak broadening in 2θ - scans. Most four common slit configuration cases are chosen. The instrumental broadening has been measured by using standard Si powder sample.
Scherrer formula:
where:
K is Scherrer constant (typically close to unity K=0.9-1)
λ is a wavelength of X-ray radiation (λ Cu-Kα1 = 1.540562 Å, and in case both Cu-Kα1 and Cu-Kα2 are present λ Cu-Kα1,2 = 1.541871 Å)
θ is Bragg angle
βsample is a peak broadening. The technical point should be noted that intergal breadth and/or FWHM have to be inserted in radians.
in the case where the peaks obey Lorentzian (or Cauchy) distribution profile.
in the case of Gaussian distribution profile.
Experimental results implied crystallite size to cause a Cauchy-type broadening while strain broadening was associated with a Gauss profile. Real measurement contains contributions of both Lorentzian (Cauchy) and Gaussian distributions.
Full scans
- 2θ scans of Si reference sample.
-
Measured Si powder reference sample with different incident slit (IS) and incident angle ω values.
- Broadening functions.
-
Calculated FWHM as a function of 2θ.
-
Calculated Integral breadth as a function of 2θ.
case1
IS=0.5 mm and ω=2°
Peak number | 2θ (°) | FWHM (°) | FWHM (rad) | Integral breadth (°) | Integral breadth (rad) |
---|---|---|---|---|---|
1 | 28.4077 | 0.2923 | 0.0051 | 0.3232 | 0.0056 |
2 | 47.2895 | 0.3109 | 0.0054 | 0.3395 | 0.0059 |
3 | 56.1274 | 0.3004 | 0.0052 | 0.3368 | 0.0059 |
4 | 69.1426 | 0.3082 | 0.0054 | 0.3325 | 0.0058 |
5 | 76.3659 | 0.2585 | 0.0045 | 0.2936 | 0.0051 |
6 | 88.0122 | 0.3174 | 0.0055 | 0.3609 | 0.0063 |
7 | 94.9581 | 0.3126 | 0.0055 | 0.3434 | 0.0060 |
8 | 106.7351 | 0.3317 | 0.0058 | 0.3637 | 0.0063 |
case2
IS=0.5 mm and ω=1°
Peak number | 2θ (°) | FWHM (°) | FWHM (rad) | Integral breadth (°) | Integral breadth (rad) |
---|---|---|---|---|---|
1 | 28.4185 | 0.2961 | 0.0052 | 0.3246 | 0.0057 |
2 | 47.2935 | 0.2961 | 0.0052 | 0.3214 | 0.0056 |
3 | 56.1085 | 0.2881 | 0.0050 | 0.3206 | 0.0056 |
4 | 69.1297 | 0.3009 | 0.0053 | 0.3203 | 0.0056 |
5 | 76.3485 | 0.3110 | 0.0054 | 0.3525 | 0.0062 |
6 | 88.0310 | 0.2972 | 0.0052 | 0.3234 | 0.0056 |
7 | 94.9806 | 0.2872 | 0.0050 | 0.3114 | 0.0054 |
8 | 106.7100 | 0.2838 | 0.0050 | 0.3024 | 0.0053 |
case3
IS=1 mm and ω=2°
Peak number | 2θ (°) | FWHM (°) | FWHM (rad) | Integral breadth (°) | Integral breadth (rad) |
---|---|---|---|---|---|
1 | 28.3469 | 0.3041 | 0.0053 | 0.3237 | 0.0056 |
2 | 47.2945 | 0.3009 | 0.0053 | 0.3242 | 0.0057 |
3 | 56.1208 | 0.3064 | 0.0053 | 0.3322 | 0.0058 |
4 | 69.1388 | 0.3363 | 0.0059 | 0.3598 | 0.0063 |
5 | 76.3682 | 0.2689 | 0.0047 | 0.3100 | 0.0054 |
6 | 88.0168 | 0.3443 | 0.0060 | 0.3811 | 0.0067 |
7 | 94.9673 | 0.3018 | 0.0053 | 0.3289 | 0.0057 |
8 | 106.7248 | 0.3344 | 0.0058 | 0.3655 | 0.0064 |
case4
IS=1 mm and ω=1°
Peak number | 2θ (°) | FWHM (°) | FWHM (rad) | Integral breadth (°) | Integral breadth (rad) |
---|---|---|---|---|---|
1 | 28.4186 | 0.2981 | 0.0052 | 0.3187 | 0.0056 |
2 | 47.2990 | 0.2998 | 0.0052 | 0.3192 | 0.0056 |
3 | 56.0990 | 0.2991 | 0.0052 | 0.3418 | 0.0060 |
4 | 69.1210 | 0.2992 | 0.0052 | 0.3318 | 0.0058 |
5 | 76.3549 | 0.3070 | 0.0054 | 0.3386 | 0.0059 |
6 | 88.0328 | 0.3053 | 0.0053 | 0.3437 | 0.0060 |
7 | 94.9712 | 0.2838 | 0.0050 | 0.3127 | 0.0055 |
8 | 106.7197 | 0.2799 | 0.0049 | 0.2980 | 0.0052 |