==A few words about the furnace==
==A few words about the furnace==
[[image:Furnace_nitride1.jpg|300x300px|right]]
[[image:Furnace_nitride1.jpg|300x300px|right|thumb|B2 Furnace LPCVD Nitride: positioned in cleanroom 2]]
The furnace is a Tempress horisontal furnace. The process is a batch process meaning you can run a batch of 25 wafers at a time. The deposition takes place at temperatures of 800-835 degrees Celsius. The reactive gases are Ammonia and dichlorsilane. The LPCVD nitride has a good step coverage and the film thickness is very uniform over the wafer. We have two standard LPCVD nitride processes: One for depositing stoichiometric nitride (Si<sub>3</sub>N<sub>4</sub>) and one for deposition of low stress nitride (SNR). To get information on how to operate the furnace please read the manual which is uploaded to LabManager.
The furnace is a Tempress horisontal furnace. The process is a batch process meaning you can run a batch of 25 wafers at a time. The deposition takes place at temperatures of 800-835 degrees Celsius. The reactive gases are Ammonia and dichlorsilane. The LPCVD nitride has a good step coverage and the film thickness is very uniform over the wafer. We have two standard LPCVD nitride processes: One for depositing stoichiometric nitride (Si<sub>3</sub>N<sub>4</sub>) and one for deposition of low stress nitride (SNR). To get information on how to operate the furnace please read the manual which is uploaded to LabManager.



Revision as of 10:02, 4 December 2007

At the moment we have one LPCVD furnace for nitride depositions.


A few words about the furnace

B2 Furnace LPCVD Nitride: positioned in cleanroom 2

The furnace is a Tempress horisontal furnace. The process is a batch process meaning you can run a batch of 25 wafers at a time. The deposition takes place at temperatures of 800-835 degrees Celsius. The reactive gases are Ammonia and dichlorsilane. The LPCVD nitride has a good step coverage and the film thickness is very uniform over the wafer. We have two standard LPCVD nitride processes: One for depositing stoichiometric nitride (Si3N4) and one for deposition of low stress nitride (SNR). To get information on how to operate the furnace please read the manual which is uploaded to LabManager.

Process Knowledge

Please take a look at the process side for deposition of Silicon Nitride using LPCVD: Deposition of Silicon Nitride using LPCVD


A rough overview of the performance of LPCVD Silicon Nitride and some process related parameters

Purpose Deposition of silicon nitride Stoichiometry:
  • Si3N4
  • SRN

SRN: Silicon Rich Nitride

Performance Film thickness
  • Si3N4:~50Å - ~3000Å
  • SRN: ~50Å - ~10000Å
Step coverage
  • Good
Film quality
  • Dense film
  • Few defects
Process parameter range Process Temperature
  • 800-835 oC
Process pressure
  • 80-230 mTorr
Gas flows
  • SiH2Cl2:10-100 sccm
  • NH3:10-75 sccm
Substrates Batch size
  • 1-25 4" wafer per run
  • deposition on both sides of the substrate
Substrate material allowed
  • Silicon wafers (new from the box or RCA cleaned)
    • with layers of silicon oxide or silicon (oxy)nitride (RCA cleaned)
  • Quartz wafers (RCA cleaned)