Specific Process Knowledge/Lithography/Descum: Difference between revisions

From LabAdviser
Jehem (talk | contribs)
Jehem (talk | contribs)
Line 170: Line 170:
=Plasma asher 3=
=Plasma asher 3=


Plasma Asher 3 is specially used for control descum process after lithography. Please notice that you only can process one 4 inch wafer or one small sampel at a time.
Plasma Asher 3 is specifically used for controlled descum process after lithography. Please note that you only can process a single 100 mm wafer, or one small sample, at a time.
Machine is equipped with 2 gaslines: oxygen and nitrogen, but all tests run with oxygen as recommended by Diener.
The plasma asher is equipped with 2 gaslines: oxygen and nitrogen, but all standard processes use only oxygen (as recommended by Diener).


'''Ashing of  AZ MiR701 resist'''


You can use different strategy planing your descum: you can change power settings or you can vary chamber pressure during descum.
'''Ashing of  AZ MiR701 resist:'''<br>
You can use two different descum process developments: you can either change power settings or processing chamber pressure.


''Testing different power settings''


[[image:AZMIR701_power_settings.png|right|frame|400x400px| Descum results for different power settings]]
'''Testing different power settings:'''
[[image:AZMIR701_power_settings.png|640px|thumb|Descum results for different power settings]]


Recipe settings:
'''Recipe settings:'''
Kept oxygen and pressure settings constant at Oxygen: 5 sccm under process; Pressure: 0,2mbar and vary power.
*O2 flow: 5 sccm
*N2 flow: 0
*Pressure: 0.2 mbar
*Power: Varied


Experiment parameters:
 
'''Experiment parameters:'''
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
Line 201: Line 205:
<br clear="all" />
<br clear="all" />


''Testing different pressure settings''


Recipe settings:
'''Testing different pressure settings:'''
Kept power setting constant at Power: 100% and vary oxygen flow during process.
[[image:AZMIR701_pressure_settings.png|640px|thumb|Descum results for different pressure settings]]


[[image:AZMIR701_pressure_settings.png|right|frame|400x400px| Descum results for different pressure settings]]
'''Recipe settings:'''
*O2 flow: varied
*N2 flow: 0
*Pressure: varied
*Power: V100% (100 W)




Experiment parameters:
'''Experiment parameters:'''
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
Line 222: Line 229:
|}
|}
|}
|}
<br clear="all" />
<br clear="all" />


'''Ashing of AZ5214E resist'''
'''Ashing of AZ5214E resist:'''
[[image:AZ5214E_pressure_settings.png|640px|thumb|Descum results for different pressure settings]]


[[image:AZ5214E_pressure_settings.png|right|frame|400x400px| Descum results for different pressure settings]]


Recipe settings:
'''Recipe settings:'''
Kept power setting constant at Power: 100% and vary oxygen flow during process.
*O2 flow: varied
*N2 flow: 0
*Pressure: varied
*Power: V100% (100 W)




Experiment parameters:
'''Experiment parameters:'''
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  

Revision as of 12:05, 30 January 2023

Feedback to this page: click here

Plasma asher 1

Descum results plasma asher 1. September 2019

The user manual(s), quality control procedure(s) and results and contact information can be found in LabManager.

Descum of AZ5214E resist on 50mm silicon wafer. Wafer was placed horisontally in chamber on a 100 mm carier wafer.


Recipe 1:
Note: Plasma asher was cold before use

  • O2 flow: 70 ml/min
  • N2 flow: 70 ml/min
  • Power: 150 W
Ashing time (min) 1 2 5 7 10 10
Etched Thickness (nm) 14.2 16.3 47.6 123.2 854.3 862.1


Recipe 2:
Note: Plasma asher was cold before use

  • O2 flow: 500 ml/min
  • N2 flow: 0 ml/min
  • Power: 500 W
Ashing time (min) 1 2 5 7 10 10
Etched Thickness (nm) - 8.1 32.9 271.1 495.6 446.2


Descum tests on UV resists

Conny Hjort & Jesper Hanberg, September 2021

Descum results plasma asher 1. August 2021

Descum of different resists, AZ5214E, AZ701 MiR and AZ2020 nLOF, on a single 100mm wafer was tested. Wafer was placed vertically in the middle of glass carrier.

Recipe settings:
Note: plasma Asher was cold before use.

  • O2 flow: 70 ml/min
  • N2 flow: 70 ml/min

Power: 150 W

Minor temperature rise during processing was observed, but not more than 5 degrees. Starting chamber pressure was around 0.5 mbar.


1,5 um AZ5214E resist:

Ashing time (min) 1 2 3 5 7
Etched Thickness (nm) 6,28 102,99 76,92 N/A N/A


1,5 um AZ5214E resist placed horizontally in the carrier:

Ashing time (min) 1 2 3 5 7
Etched Thickness (nm) 63,03 143,32 304,29 372,59 N/A


1,5 um AZ701MiR resist:

Ashing time (min) 1 2 3 5 7
Etched Thickness (nm) 268,88 199,54 219,03 200,86 292,15


1,5 um AZ 2020nLOF resist:

Ashing time (min) 1 2 3 5 7
Etched Thickness (nm) 1,68 76,51 169,72 481,96 272,59


Plasma asher 2

Jitka Urbánková & Jesper Hanberg, December 2019

Descum results plasma asher 2 - recipe 1

The user manual(s), quality control procedure(s) and results and contact information can be found in LabManager.

Descum of AZ Mir 701 resist on 100mm silicon wafer. Five wafers were placed vertically in chamber.


recipe 1:

  • O2 flow: 100 ml/min
  • N2 flow: 100 ml/min
  • Power: 150 W
Ashing time (min) 1 2 3 4 6 7 8 9 10 12 14 15 20
Etched Thickness (nm) 8,7 5,1 12,5 6,2 31,8 86,0 25,7 46,8 38,3 49,7 59,4 140,1 360,7
Initial temperature (°C) 28 21 31 21 22 28 25 24 21 24 24 22 22
Descum results plasma asher 2 - recipe 2


recipe 2:

  • O2 flow: 500 ml/min
  • N2 flow: 0 ml/min
  • Power: 200 W
Ashing time (min) 1 2 3 4 5 6 7 8 10 12 15 20
Etched Thickness (nm) 8,1 9,4 16,8 55,2 44,0 47,5 42,5 55,1 85,3 122,4 184,8 305,9
Initial temperature (°C) 22 21 21 22 22 22 21 21 20 21 21 22

A linear time dependence was observed after etching 7 minutes or more (recipe 2).

Plasma asher 3

Plasma Asher 3 is specifically used for controlled descum process after lithography. Please note that you only can process a single 100 mm wafer, or one small sample, at a time. The plasma asher is equipped with 2 gaslines: oxygen and nitrogen, but all standard processes use only oxygen (as recommended by Diener).


Ashing of AZ MiR701 resist:
You can use two different descum process developments: you can either change power settings or processing chamber pressure.


Testing different power settings:

Descum results for different power settings

Recipe settings:

  • O2 flow: 5 sccm
  • N2 flow: 0
  • Pressure: 0.2 mbar
  • Power: Varied


Experiment parameters:

FW/REV C2/C1 Power
recipe 1 50/0 52/31 50%
recipe 2 100/0 53/31 100%
recipe 3 20/0 51/34 20%



Testing different pressure settings:

Descum results for different pressure settings

Recipe settings:

  • O2 flow: varied
  • N2 flow: 0
  • Pressure: varied
  • Power: V100% (100 W)


Experiment parameters:

FW/REV C2/C1 Oxygen Pressure
recipe 1 100/0 53/31 5 0,2
recipe 2 100/0 37/38 45 0,8


Ashing of AZ5214E resist:

Descum results for different pressure settings


Recipe settings:

  • O2 flow: varied
  • N2 flow: 0
  • Pressure: varied
  • Power: V100% (100 W)


Experiment parameters:

FW/REV C2/C1 Oxygen Pressure
recipe 1 100/0 53/31 17 0,4
recipe 2 100/0 37/39 45 0,8