Jump to content

Specific Process Knowledge/Lithography/Strip: Difference between revisions

From LabAdviser
Jehem (talk | contribs)
No edit summary
Jehem (talk | contribs)
 
Line 61: Line 61:
! scope=row style="text-align: left;" | Process pressure
! scope=row style="text-align: left;" | Process pressure
| 0.8 mbar
| 0.8 mbar
| 0.5-1.5 mbar
| 0.5-1.5 mbar<br>(standard process 1.3 mbar)
| 0.5-1.5 mbar
| 0.5-1.5 mbar<br>(standard process 1.3 mbar)
| NA
| NA
| NA
| NA

Latest revision as of 08:57, 21 September 2026

The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.

Feedback to this page: click here

Strip Comparison Table

Plasma Asher 3: Descum Plasma Asher 4 (Clean) Plasma Asher 5 (Dirty) Resist strip Lift-off
Purpose Resist descum
  • Resist stripping
  • Resist descum
  • Surface treatment
  • Other ashing of organic material
  • Resist stripping
  • Resist descum
  • Surface treatment
  • Other ashing of organic material
Resist stripping Metal lift-off
Method Plasma ashing Plasma ashing Plasma ashing Solvent & ultrasonication Solvent & ultrasonication
Process gasses O2 (50 sccm)
  • O2 (0-500 sccm)
  • N2 (0-500 sccm)
  • O2 (0-500 sccm)
  • N2 (0-500 sccm)
  • CF4 (0-200 sccm)
NA NA
Process power 10-100 W (10-100%) 150-1000 W 150-1000 W NA NA
Process pressure 0.8 mbar 0.5-1.5 mbar
(standard process 1.3 mbar)
0.5-1.5 mbar
(standard process 1.3 mbar)
NA NA
Process solvent NA NA NA
  • NMP (Remover 1165)
  • IPA (rinsing agent)
  • NMP (Remover 1165)
  • IPA (rinsing agent)
Process temperature Up to ~100°C Up to ~100°C Up to ~100°C Up to ~65°C Up to ~65°C
Process time 1-10 minutes
  • Stripping: 20-90 minutes
  • Descum: 5-15 minutes
  • Surface treatment: Seconds to minutes
  • Other ashing: Hours, material dependent
  • Stripping: 20-90 minutes
  • Descum: 5-15 minutes
  • Surface treatment: Seconds to minutes
  • Other ashing: Hours, material dependent
  • NMP (Remover 1165)
  • IPA (rinsing agent)
  • NMP (Remover 1165)
  • IPA (rinsing agent)
Substrate batch
  • Chips: several
  • 50 mm wafer: several
  • 100 mm wafer: 1
  • Chips: several
  • 50 mm wafer: several
  • 100 mm wafer: 1-25
  • 150 mm wafer: 1-25
  • 200 mm wafer: 1-25
  • Chips: several
  • 50 mm wafer: several
  • 100 mm wafer: 1-25
  • 150 mm wafer: 1-25
  • 200 mm wafer: 1-25
  • 100 mm wafer: 1-25
  • 150 mm wafer: 1-25
  • 100 mm wafer: 1-25
  • 150 mm wafer: 1-25
Substrate materials
  • No polymer substrates
  • Silicon substrates
  • III-V substrates
  • Glass substrates
  • Films, or patterned films, of any material except type IV (Pb, Te)
  • No metals
  • No metal oxides
  • No III-V materials
  • Silicon substrates
  • Glass substrates
  • Polymer substrates
  • Films, or patterned films, of resists/polymers
  • Silicon substrates
  • III-V substrates (only on Si carrier)
  • Glass substrates
  • Polymer substrates
  • Films, or patterned films, of any material except type IV (Pb, Te)
  • No iron (Fe) containing films
  • Silicon substrates
  • III-V substrates
  • Glass substrates
  • Polymer substrates
  • Films, or patterned films, of any material except type IV (Pb, Te)
  • No iron (Fe) or Copper (Cu) containing films
  • Silicon substrates
  • III-V substrates (only if clean)
  • Glass substrates
  • Films, or patterned films, of any material except type IV (Pb, Te)

Decommisioned tools

Plasma asher 1 was decommissioned 2024-12-02.

Information about decommissioned tool can be found here.


Plasma asher 2 was decommissioned 2024-12-02.

Information about decommissioned tool can be found here.