= Strip Comparison Table =
= Strip Comparison Table =
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"
{| class="wikitable"
 
|-
!colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment
!
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Strip#Plasma Asher 3: Descum|Plasma Asher 3: Descum]]</b>
! [[Specific_Process_Knowledge/Lithography/Strip/plasmaAsher03|Plasma Asher 3: Descum]]
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Strip#Plasma_Asher_4|Plasma Asher 4]]</b>
! [[Specific_Process_Knowledge/Lithography/Strip/plasmaAsher04|Plasma Asher 4 (Clean)]]
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Strip#Plasma Asher 5|Plasma Asher 5]]</b>
! [[Specific_Process_Knowledge/Lithography/Strip/plasmaAsher05|Plasma Asher 5 (Dirty)]]
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Strip#Resist Strip|Resist strip]]</b>
! [[Specific_Process_Knowledge/Lithography/Strip/resistStrip|Resist strip]]
|style="background:WhiteSmoke; color:black"|<b>[[Specific Process Knowledge/Lithography/LiftOff|Lift-off]]</b>
! [[Specific Process Knowledge/Lithography/LiftOff|Lift-off]]
 
|-
|-
!style="background:silver; width:100px; color:black;" align="center"|Purpose  
! scope=row style="text-align: left;" | Purpose  
|style="background:LightGrey; color:black"|
| Resist descum
|style="background:WhiteSmoke; color:black"|
|
Resist descum
*Resist stripping
|style="background:WhiteSmoke; color:black"|
*Resist descum
Clean wafers only, no metal
*Surface treatment
|style="background:WhiteSmoke; color:black"|
*Other ashing of organic material
All purposes
|
|style="background:WhiteSmoke; color:black"|
*Resist stripping
Resist strip, no metal lift off
*Resist descum
|style="background:WhiteSmoke; color:black"|
*Surface treatment
Lift-off
*Other ashing of organic material
 
| Resist stripping
| Metal lift-off
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="1"|Method
! scope=row style="text-align: left;" | Method
|style="background:LightGrey; color:black"|
| Plasma ashing
|style="background:WhiteSmoke; color:black"|
| Plasma ashing
Plasma ashing
| Plasma ashing
|style="background:WhiteSmoke; color:black"|
| Solvent & ultrasonication
Plasma ashing
| Solvent & ultrasonication
|style="background:WhiteSmoke; color:black"|
Plasma ashing
|style="background:WhiteSmoke; color:black"|
Solvent and ultra sound
|style="background:WhiteSmoke; color:black"|
Solvent and ultra sound
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameters
! scope=row style="text-align: left;" | Process gasses
|style="background:LightGrey; color:black"|Process gasses
| O<sub>2</sub> (50 sccm)
|style="background:WhiteSmoke; color:black"|
|
*O<sub>2</sub> (flow unknown)
|style="background:WhiteSmoke; color:black"|
*O<sub>2</sub> (0-500 sccm)
*O<sub>2</sub> (0-500 sccm)
*N<sub>2</sub> (0-500 sccm)
*N<sub>2</sub> (0-500 sccm)
|style="background:WhiteSmoke; color:black"|
|
*O<sub>2</sub> (0-500 sccm)
*O<sub>2</sub> (0-500 sccm)
*N<sub>2</sub> (0-500 sccm)
*N<sub>2</sub> (0-500 sccm)
*CF<sub>4</sub> (0-200 sccm)
*CF<sub>4</sub> (0-200 sccm)
|style="background:WhiteSmoke; color:black"|
| NA
*NA
| NA
|style="background:WhiteSmoke; color:black"|
|-
*NA
! scope=row style="text-align: left;" | Process power
 
| 10-100 W (10-100%)
| 150-1000 W
| 150-1000 W
| NA
| NA
|-
|-
|style="background:LightGrey; color:black"|Max. process power
! scope=row style="text-align: left;" | Process pressure
|style="background:WhiteSmoke; color:black"|
| 0.8 mbar
100 W (100%)
| 0.5-1.5 mbar<br>(standard process 1.3 mbar)
|style="background:WhiteSmoke; color:black"|
| 0.5-1.5 mbar<br>(standard process 1.3 mbar)
1000 W
| NA
|style="background:WhiteSmoke; color:black"|
| NA
1000 W
|style="background:WhiteSmoke; color:black"|
*NA
|style="background:WhiteSmoke; color:black"|
*NA
 
|-
|-
|style="background:LightGrey; color:black"|Solvent
! scope=row style="text-align: left;" | Process solvent
|style="background:WhiteSmoke; color:black"|
| NA
*NA
| NA
|style="background:WhiteSmoke; color:black"|
| NA
*NA
|
|style="background:WhiteSmoke; color:black"|
*NA
|style="background:WhiteSmoke; color:black"|
*NMP (Remover 1165)
*NMP (Remover 1165)
*Rinse in IPA
*IPA (rinsing agent)
|style="background:WhiteSmoke; color:black"|
|
*NMP (Remover 1165)
*NMP (Remover 1165)
*Rinse in IPA
*IPA (rinsing agent)
 
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
! scope=row style="text-align: left;" | Process temperature
|style="background:LightGrey; color:black"|Batch size
| Up to ~100°C
|style="background:WhiteSmoke; color:black"|
| Up to ~100°C
*1 small sample
| Up to ~100°C
*1 50 mm wafer
| Up to ~65°C
*1 100 mm wafer
| Up to ~65°C
|style="background:WhiteSmoke; color:black"|
*1 small sample
*1 50 mm wafer
*1-25 100 mm wafers
*1-25 150 mm wafers
*1-25 200 mm wafers
|style="background:WhiteSmoke; color:black"|
*1 small sample
*1 50 mm wafer
*1-25 100 mm wafers
*1-25 150 mm wafers
*1-25 200 mm wafers
|style="background:WhiteSmoke; color:black"|
*1 - 25 100 mm wafers
*1 - 25 150 mm wafers
|style="background:WhiteSmoke; color:black"|
*1 - 25 100 mm wafers
*1 - 25 150 mm wafers
|-
|-
|style="background:LightGrey; color:black"|Allowed materials
! scope=row style="text-align: left;" | Process time
|style="background:WhiteSmoke; color:black"|
| 1-10 minutes
*Silicon, glass, and polymer substrates
|  
*Film or pattern of all but Type IV
*Stripping: 20-90 minutes
|style="background:WhiteSmoke; color:black"|
*Descum: 5-15 minutes
*<b>No metals allowed - including metal oxides</b><br>
*Surface treatment: Seconds to minutes
*<b>No III-V materials</b>
*Other ashing: Hours, material dependent
*Silicon, glass, and polymer substrates
|  
*Film or pattern of photoresist/polymer
*Stripping: 20-90 minutes
|style="background:WhiteSmoke; color:black"|
*Descum: 5-15 minutes
*Silicon, III-V, and glass substrates
*Surface treatment: Seconds to minutes
*Film or pattern of all but Type IV
*Other ashing: Hours, material dependent
|style="background:WhiteSmoke; color:black"|
|
*<b>No metals allowed - including metal oxides</b><br>
*NMP (Remover 1165)
*Silicon, glass, and polymer substrates
*IPA (rinsing agent)
*Film or pattern of photoresist/polymer
|
|style="background:WhiteSmoke; color:black"|
*NMP (Remover 1165)
*Silicon and glass substrates
*IPA (rinsing agent)
*Film or pattern of all but Type IV
|-
|}
 
<br clear="all" />
 
= Plasma Ashing =
 
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"
|-
|-
 
! scope=row style="text-align: left;" | Substrate batch
|-style="background:silver; color:black"
|
*Chips: several
*50 mm wafer: several
*100 mm wafer: 1
|
*Chips: several
*50 mm wafer: several
*100 mm wafer: 1-25
*150 mm wafer: 1-25
*200 mm wafer: 1-25
|
*Chips: several
*50 mm wafer: several
*100 mm wafer: 1-25
*150 mm wafer: 1-25
*200 mm wafer: 1-25
|
*100 mm wafer: 1-25
*150 mm wafer: 1-25
|
|
! Photoresist stripping
*100 mm wafer: 1-25
! [[Specific_Process_Knowledge/Lithography/Descum|Descum after lithography]]
*150 mm wafer: 1-25
! Surface treatment of plastic, ceramic and metal
! Ashing of organic material
|-
 
|-style="background:whitesmoke; color:black"
!Process pressure
|0.5-1.5 mbar
|0.5-1.5 mbar
|0.5-1.5 mbar
|0.5-1.5 mbar
|-
|-
 
! scope=row style="text-align: left;" | Substrate materials
|-style="background:silver; color:black"
|
!Process gases
*<span style="color:red">'''No polymer substrates'''</span><br>
*Silicon substrates
*III-V substrates
*Glass substrates
*Films, or patterned films, of any material except type IV (Pb, Te)
|
*<span style="color:red">'''No metals'''</span><br>
*<span style="color:red">'''No metal oxides'''</span><br>
*<span style="color:red">'''No III-V materials'''</span><br>
*Silicon substrates
*Glass substrates
*Polymer substrates
*Films, or patterned films, of resists/polymers
|
*Silicon substrates
*III-V substrates (only on Si carrier)
*Glass substrates
*Polymer substrates
*Films, or patterned films, of any material except type IV (Pb, Te)
|
|
*O<sub>2</sub> (140 sccm)
*<span style="color:red">'''No iron (Fe) containing films'''</span>
*N<sub>2</sub> (60 sccm)
*Silicon substrates
*III-V substrates
*Glass substrates
*Polymer substrates
*Films, or patterned films, of any material except type IV (Pb, Te)
|
|
*O<sub>2</sub> (70-210 sccm)
*<span style="color:red">'''No iron (Fe) or Copper (Cu) containing films'''</span>
*N<sub>2</sub> (0-70 sccm)
*Silicon substrates
|O<sub>2</sub>, CF<sub>4</sub>, N<sub>2</sub> or their mixtures
*III-V substrates (only if clean)
|O<sub>2</sub>
*Glass substrates
|-
*Films, or patterned films, of any material except type IV (Pb, Te)
 
|-style="background:whitesmoke; color:black"
!Process  power
|1000 W
|150-1000 W
|150-1000 W
|1000 W or less for heat- sensitive materials
|-
 
|-style="background:silver; color:black"
!Process  time
|5-90 minutes
|1-10 minutes
|seconds to minutes
|Between 0.5 and 20 hours, depending on the material
|-
 
|-style="background:whitesmoke; color:black"
!Batch size
|1-25
|1-25
|1 wafer at a time
|1 wafer at a time, use a container, e.g Petri dish
|-
|}
|}


<br clear="all" />
=Decommisioned tools=
 
<!--
Typical process time for stripping in plasma asher 1 or 2:
*1.5 µm AZ 5214E resist film: ~15 min
*10 µm AZ 4562 resist film: ~45 min
 
Typical process parameters:
*O<sub>2</sub>: 400 ml/min
*N<sub>2</sub>: 70 ml/min
*Power: 1000 W
 
 
A typical descum process in plasma asher 1 or 2:
*O<sub>2</sub>: 70 ml/min
*N<sub>2</sub>: 70 ml/min
*Power: 150 W
*Time : 10 min
 
 
Be sure to wait for chamber to cool down to room temperature, before runinng descum processes in plasma asher 1 or 2. At a load of 2 Fused silica wafers, the amount of resist removed will be 10 - 1500 nm.
 
'''NB: Use dedicated descum asher Plasma Asher 3: Descum for descumming.'''
-->
 
==Process gas ratio for plasma asher 4 & 5==
[[File:PA_gas_mix_v2.png|320px|thumb|Ashing rate as function of gas mix ratio.|right]]
The ashing rate is related to the gas mix, usually expressed as percentage of nitrogen of the total amount of gas.
 
Test using a single 100 mm wafer in the center of the process chamber shows that 30-80% nitrogen gives the highest ashing rate.
 
<b>Test parameters:</b><br>
Total gas flow rate: 500 sccm<br>
Gas mix ratio: tested parameter<br>
DSC: not used for this test<br>
Chamber pressure: 1.2 mbar<br>
Power: 1000 W<br>
Processing time: 2 minutes<br>
Temperature (average): 43°C
<br clear="all" />
 
==Process chamber pressure for plasma asher 4 & 5==
[[File:PA_chamber_pressure_v2.png|320px|thumb|Ashing rate as function of chamber pressure.|right]]
The ashing rate is related to the chamber pressure during processing.
 
Test using a single 100 mm wafer in the center of the process chamber shows that a chamber pressure of 1.3 mbar gives the highest ashing rate.
 
<b>Test parameters:</b><br>
Total gas flow rate: 150 sccm<br>
Gas mix ratio: 30% nitrogen<br>
DSC: tested parameter<br>
Chamber pressure: tested parameter<br>
Power: 1000 W<br>
Processing time: 2 minutes<br>
Temperature (average): 43°C
<br clear="all" />
 
==Process gas flow rate for plasma asher 4 & 5==
[[File:PA_flowRate_v3.png|320px|thumb|Ashing rate as function of total gas flow rate.|right]]
The ashing rate is related to the total gas flow rate during processing.
 
Test using a single 100 mm wafer in the center of the process chamber shows that a total flow rate of 200 sccm gives the highest ashing rate.
 
<b>Test parameters:</b><br>
Total gas flow rate: tested parameter<br>
Gas mix ratio: 30% nitrogen<br>
DSC: 1.3 mbar<br>
Chamber pressure: 1.3 mbar<br>
Power: 1000 W<br>
Processing time: 2 minutes<br>
Temperature (average): 43°C
<br clear="all" />
 
==Process power for plasma asher 4 & 5==
[[File:PA_power_v1.png|320px|thumb|Ashing rate as function of microwave power.|right]]
The ashing rate is related to the power used during processing. Higher power gives higher ashing rate. <span style="color:red">There is an unexpected peak at 800 W which we will investigate further.</span>
 
Test using a single 100 mm wafer in the center of the process chamber shows that a power of 1000 W gives the highest ashing rate.
 
<b>Test parameters:</b><br>
Total gas flow rate: 200 sccm<br>
Gas mix ratio: 30% nitrogen<br>
DSC: 1.3 mbar<br>
Chamber pressure: 1.3 mbar<br>
Power: tested parameter<br>
Processing time: 2 minutes<br>
Temperature (average): 43°C
<br clear="all" />
 
==Process temperature for plasma asher 4 & 5==
[[File:PA_temperature_v1.png|320px|thumb|Ashing rate as function of temperature.|right]]
The ashing rate is related to the temperature during processing. Higher temperature gives higher ashing rate.
 
Test using a single 100 mm wafer in the center of the process chamber shows that increasing processing temperature gives increasing ashing rate.
 
<b>Test parameters:</b><br>
Total gas flow rate: 200 sccm<br>
Gas mix ratio: 30% nitrogen<br>
DSC: 1.3 mbar<br>
Chamber pressure: 1.3 mbar<br>
Power: 1000 W<br>
Processing time: 2 minutes<br>
Temperature (average): tested parameter
<br clear="all" />
 
 
==Plasma Asher 1==
<span style="color:red">Plasma asher 1 was decommissioned 2024-12-02.</span>
<span style="color:red">Plasma asher 1 was decommissioned 2024-12-02.</span>


[[Specific Process Knowledge/Lithography/Strip/PlasmaAsher1|Information about decommissioned tool can be found here.]]
[[Specific Process Knowledge/Lithography/Strip/PlasmaAsher1|Information about decommissioned tool can be found here.]]


==Plasma Asher 2==
 
<span style="color:red">Plasma asher 2 was decommissioned 2024-12-02.</span>
<span style="color:red">Plasma asher 2 was decommissioned 2024-12-02.</span>


[[Specific Process Knowledge/Lithography/Strip/PlasmaAsher2|Information about decommissioned tool can be found here.]]
[[Specific Process Knowledge/Lithography/Strip/PlasmaAsher2|Information about decommissioned tool can be found here.]]
==Plasma Asher 3: Descum==
[[image:2017-03-15 13.12.45.jpg|350x350px|thumb|Plasma Asher 3: Descum is placed A-5]]
The Plasma Asher 3: Descum dedicated for resist descum i.e. removal of remains resist traces after development. It has a small chamber, so you can only load a single 100 mm substrate or a few smaller pieces.
In this machine, only O2 and N2 gases are used for processes.
<b>Typical process parameters when operating the equipment:</b><br>
Process: Photoresist descum<br>
Pressure: 0.2-0.8 mbar<br>
Gas: O<sub>2</sub><br>
Power: 50-100%<br>
Time:1 -10 minutes (depending on photoresist type and thickness)<br>
The other materials have not been tested yet.
The user manual, user APV, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=423 LabManager] - '''requires login'''
===Process Information===
Detailed information about descum processing on Plasma asher 3: Descum can be found [[Specific Process Knowledge/Lithography/Descum|here]].
<br clear="all" />
<!-- TARAN 220-03-05
==III-V Plasma Asher==
[[Image:III-V_asher.jpg|300x300px|thumb|Plasma asher for removing resist on III-V samples: positioned in A-5]]
Diener Pico Plasma Asher for III-V materials.
The user manual and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=186 LabManager] - '''requires login'''
<br clear="all" />
-->
=Plasma Asher 4=
[[File:PA5 front.jpg|320px|thumb|Plasma asher 4 in cleanroom E-5.|right]]
The Plasma Asher 4 can be used for the following processes:
*Photoresist stripping
*Descumming
*Surface cleaning
*Removal of organic passivation layers and masks
Plasma asher 4 has the following material restrictions:
*No metals allowed
*No metal oxides allowed
*No III-V materials allowed
The user manual, risk assessment, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=530 LabManager] - '''requires login'''
===Process Information===
*[[Specific Process Knowledge/Lithography/Descum#Plasma Asher 4|Descum using plasma asher 4]]
'''Typical stripping parameters'''
*Resist: 1.5 µm AZ 5214E
*Substrate: 100 mm Si
*O<sub>2</sub>: 140 sccm
*N<sub>2</sub>: 60 sccm
*Pressure (DSC): 1.3 mbar
*Power: 1000 W
*Time (single wafer): 20 minutes
*Time (full boat): 90 minutes
The user manual, user APV, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=200 LabManager] - '''requires login'''
===Process Information===
*[[Specific Process Knowledge/Lithography/Descum|Descum]]
<br clear="all" />
=Plasma Asher 5=
[[File:PA5 front.jpg|320px|thumb|Plasma asher 5 in cleanroom E-5.|right]]
The Plasma Asher 5 can be used for the following processes:
*Photoresist stripping
*Descumming
*Surface cleaning
*Removal of organic passivation layers and masks
Furthermore plasma processing using CF<sub>4</sub> in plasma asher 5 can be used for:
*Etching of glass and ceramic
*Etching of SiO<sub>2</sub>, Si<sub>3</sub>N<sub>4</sub>, Si
*Removal of polyimide layers
'''Typical stripping parameters'''
*Resist: 1.5 µm AZ 5214E
*Substrate: 100 mm Si
*O<sub>2</sub>: 140 sccm
*N<sub>2</sub>: 60 sccm
*Pressure (DSC): 1.3 mbar
*Power: 1000 W
*Time (single wafer): 20 minutes
*Time (full boat): 90 minutes
Plasma asher 5 can be used for almost every material, but if you have any doubt if your materials are compatible/allowed in plasma asher 5, feel free to ask the lithography group at Nanolab.
The user manual, risk assessment, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=531 LabManager] - '''requires login'''
===Process Information===
*[[Specific Process Knowledge/Etch/Etching of Silicon Oxide/SiO2 etch using Plasma Asher |SiO<sub>2</sub> etch using Plasma Asher 5]]
*[[Specific Process Knowledge/Lithography/Descum#Plasma Asher 5|Descum using plasma asher 5]]
<br clear="all" />
=Resist Strip=
[[Image:Resist_strip.jpg|300x300px|thumb|Resist strip bench in D-3]]
This resist strip is only for wafers without metal and SU-8.
There are one Remover 1165 bath for stripping and one IPA bath for rinsing.
'''Here are the main rules for resist strip use:'''
*Place the wafers in a wafer holder and put them in the first bath for 10 min, this time is depending how much resist you have on the surface.
*After the strip rinse your wafers in the IPA bath for 2-3 min.
*Rinse your wafers for 4-5 min. in running water after stripping.
The user manual and contact information can be found in LabManager: [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=385 Resist Strip] - '''requires login'''
<br clear="all" />
<br clear="all" />
==Overview of wet bench 06 and 07==
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"
|-style="background:silver; color:black"
|
! [[Specific Process Knowledge/Lithography/Strip#Resist_Strip|Resist Strip]]
! [[Specific Process Knowledge/Lithography/LiftOff#Lift-off_wet_bench_07|Lift-off]]
|-
|-style="background:whitesmoke; color:black"
!General description'''
|Wet stripping of resist
|Lift-off process
|-
|-style="background:silver; color:black"
!Chemical solution
|NMP Remover 1165
|NMP Remover 1165
|-
|-style="background:whitesmoke; color:black"
!Process temperature
|Up to 65°C
|Up to 65°C
|-
|-style="background:silver; color:black"
!Batch size
|
1 - 25 wafers
|
1 - 25 wafers
|-
|-style="background:whitesmoke; color:black"
!Size of substrate
|
*100 mm wafers
*150 mm wafers
|
*100 mm wafers
*150 mm wafers
|-
|-style="background:silver; color:black"
!Allowed materials
|
*Silicon
*Silicon Oxide
*Silicon Nitride
*Silicon Oxynitride
|
All metals except Type IV (Pb, Te)
|-
|}

Latest revision as of 08:57, 21 September 2026

The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.

Feedback to this page: click here

Strip Comparison Table

Plasma Asher 3: Descum Plasma Asher 4 (Clean) Plasma Asher 5 (Dirty) Resist strip Lift-off
Purpose Resist descum
  • Resist stripping
  • Resist descum
  • Surface treatment
  • Other ashing of organic material
  • Resist stripping
  • Resist descum
  • Surface treatment
  • Other ashing of organic material
Resist stripping Metal lift-off
Method Plasma ashing Plasma ashing Plasma ashing Solvent & ultrasonication Solvent & ultrasonication
Process gasses O2 (50 sccm)
  • O2 (0-500 sccm)
  • N2 (0-500 sccm)
  • O2 (0-500 sccm)
  • N2 (0-500 sccm)
  • CF4 (0-200 sccm)
NA NA
Process power 10-100 W (10-100%) 150-1000 W 150-1000 W NA NA
Process pressure 0.8 mbar 0.5-1.5 mbar
(standard process 1.3 mbar)
0.5-1.5 mbar
(standard process 1.3 mbar)
NA NA
Process solvent NA NA NA
  • NMP (Remover 1165)
  • IPA (rinsing agent)
  • NMP (Remover 1165)
  • IPA (rinsing agent)
Process temperature Up to ~100°C Up to ~100°C Up to ~100°C Up to ~65°C Up to ~65°C
Process time 1-10 minutes
  • Stripping: 20-90 minutes
  • Descum: 5-15 minutes
  • Surface treatment: Seconds to minutes
  • Other ashing: Hours, material dependent
  • Stripping: 20-90 minutes
  • Descum: 5-15 minutes
  • Surface treatment: Seconds to minutes
  • Other ashing: Hours, material dependent
  • NMP (Remover 1165)
  • IPA (rinsing agent)
  • NMP (Remover 1165)
  • IPA (rinsing agent)
Substrate batch
  • Chips: several
  • 50 mm wafer: several
  • 100 mm wafer: 1
  • Chips: several
  • 50 mm wafer: several
  • 100 mm wafer: 1-25
  • 150 mm wafer: 1-25
  • 200 mm wafer: 1-25
  • Chips: several
  • 50 mm wafer: several
  • 100 mm wafer: 1-25
  • 150 mm wafer: 1-25
  • 200 mm wafer: 1-25
  • 100 mm wafer: 1-25
  • 150 mm wafer: 1-25
  • 100 mm wafer: 1-25
  • 150 mm wafer: 1-25
Substrate materials
  • No polymer substrates
  • Silicon substrates
  • III-V substrates
  • Glass substrates
  • Films, or patterned films, of any material except type IV (Pb, Te)
  • No metals
  • No metal oxides
  • No III-V materials
  • Silicon substrates
  • Glass substrates
  • Polymer substrates
  • Films, or patterned films, of resists/polymers
  • Silicon substrates
  • III-V substrates (only on Si carrier)
  • Glass substrates
  • Polymer substrates
  • Films, or patterned films, of any material except type IV (Pb, Te)
  • No iron (Fe) containing films
  • Silicon substrates
  • III-V substrates
  • Glass substrates
  • Polymer substrates
  • Films, or patterned films, of any material except type IV (Pb, Te)
  • No iron (Fe) or Copper (Cu) containing films
  • Silicon substrates
  • III-V substrates (only if clean)
  • Glass substrates
  • Films, or patterned films, of any material except type IV (Pb, Te)

Decommisioned tools

Plasma asher 1 was decommissioned 2024-12-02.

Information about decommissioned tool can be found here.


Plasma asher 2 was decommissioned 2024-12-02.

Information about decommissioned tool can be found here.