Jump to content

Specific Process Knowledge/Wafer cleaning/RCA: Difference between revisions

From LabAdviser
BGE (talk | contribs)
Hvje (talk | contribs)
Added info about cleaning non standard size samples
 
(42 intermediate revisions by 9 users not shown)
Line 1: Line 1:
{{cc-nanolab}}
'''Feedback to this page''': '''[mailto:wetchemistry@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Wafer_cleaning/RCA click here]'''
'''All links to Kemibrug (SDS) and Labmanager Including APV requires login.'''
==RCA cleaning==
==RCA cleaning==
[[Image:RCA_bench_cleanroom_2.jpg|300x300px|thumb|RCA bench: positioned in cleanroom 2. <br /> RCA1 - RCA2 - HF - ?]]
[[Image:RCA-bænk_RR2_0.JPG|300x300px|thumb|RCA bench: positioned in cleanroom B1. <br /> RCA1 - RCA2 - HF - BHF(pre-dep wafers)]]
 
The RCA cleaning procedure was originally developed by the Radio Corporation of America (RCA) as part of manufacturing electron tube components. This process has since been adapted to silicon semiconductor processing. RCA is a two-step process (RCA1 and RCA2, sometimes referred to as SC-1 and SC-2 (Standard Clean)), and RCA1 should always be made before RCA2 because removing organic contaminants is a requirement before metal contaminants can be removed effectively.<br>
 
RCA1 is a powerful oxidizer and will thus remove organic contaminants. The ammonium hydroxide in RCA1 also has good solvating power as it can complex metals such as Cu, Ag, Ni, Co and Cd into solution. RCA2 forms soluble complexes with heavy metals and also shows cleaning action similar to that of piranha solutions. Furthermore, solutions of hydrochloric acid, which is a major constituent of RCA2, has proven effective at removing alkali metal ions. RCA2 is also effective at removing metal hydroxide traces that cannot be removed in ammonia-containing solutions such as RCA1. These include Al(OH)<sub>3</sub>, Fe(OH)<sub>3</sub>, Mg(OH)<sub>2</sub> and Zn(OH)<sub>2</sub>. It is important that the chemicals used are very clean. RCA mixtures are therefore only used shortly after mixing and for a limited number of samples.<br>
 
Since RCA1 can oxidize silicon to silicon dioxide, an HF dip is sometimes used between RCA1 and RCA2. This will also remove contaminants that can be trapped in the formed oxide. However, this step is often omitted, since RCA1 removes the native oxide and then re-oxidizes the surface. This in itself has a cleaning action. It is generally not advised to do an HF dip after RCA-2 if the samples will be processed by wet chemical processes afterwards. This is because the hydrogenated surface will be extremely reactive and therefore attract contaminants from both the air and processing liquids. In this case it is better to continue processing with the passivated oxide surface. RCA clean is often done prior to furnace processes, an in these cases an HF dip after RCA-2 makes sense. Ideally the wafers should be transferred to the furnace immediately after RCA cleaning, because the samples will be very sensitive to recontamination as mentioned above.<br>


The RCA clean is used for cleaning the wafers before taking them into the furnaces and a few other equipments (check the cross contamination sheet).
A crucial part of the RCA cleaning procedure is the oxidation by H<sub>2</sub>O<sub>2</sub> at elevated temperatures. Therefore, the lifetime of RCA1 and RCA2 solutions is limited to about 1 hour after preparation and heating to 70<sup>o</sup>C because H<sub>2</sub>O<sub>2</sub> decomposes at this temperature. A temperature of 70°C is optimal. RCA solutions should never be heated above 80°C since this will lead to excessive decomposition and loss of NH<sub>3</sub>.<br>
It consists of two solutions: RCA1 and RCA2 plus diluted HF. A crucial part of the RCA clean is the oxidation by H<math>_2</math>O<math>_2</math>. Therefore the life time of the RCA solutions are limited by the presence of the H<math>_2</math>O<math>_2</math> which is highly volatile at 70 <sup>o</sup>C.


*The RCA1 contains: H<math>_2</math>O, NH<math>_4</math>OH and H<math>_2</math>O<math>_2</math> (5:1:1). It is used for removal of light organics, particles and metal. <br \>
*RCA1 contains: H<sub>2</sub>O, NH<sub>4</sub>OH and H<sub>2</sub>O<sub>2</sub> (5:1:1). It is used for removal of light organics, particles and metals.<br>
*The RCA2 contains: H<math>_2</math>O, HCl and H<math>_2</math>O<math>_2</math> (5:1:1). It is used for removal of heavy metals, alkalies and metal hydroxides.
*RCA2 contains: H<sub>2</sub>O, HCl and H<sub>2</sub>O<sub>2</sub> (5:1:1). It is used for removal of heavy metals, metal hydroxides, and residual metals including alkali metals.<br>


===RCA procedure===
You can find the APV for the RCA bench [http://labmanager.dtu.dk/d4Show.php?id=1916&mach=243 here]
*RCA1: 10 min
 
=== RCA procedure ===
*'''RCA1: 10 min'''
*DI water rinsing (dumping three times)
*DI water rinsing (dumping three times)
*HF: 30 sec (avoid it if you have oxide as the top layer)
*Optional: HF: 30 sec (you may avoid this step in case of a very thin oxide (0-200 Å) as the top layer)
*DI water rinsing (bubbler)<br>
*'''RCA2: 10 min'''
*DI water rinsing (dumping three times)
*DI water rinsing (dumping three times)
*RCA2: 10 min
*Optional: HF: 30 sec (avoid it if you have a very thin oxide (0-200 Å) as the top layer)
*DI water rinsing (dumping three times)
*DI water rinsing (bubbler)<br>
*Optional: HF: 30 sec (avoid it if you have oxide as the top layer)
For procedure details please look in the [http://labmanager.dtu.dk/d4Show.php?id=1633&mach=243 user manual] in LabManager.
*DI water rinsing (dumping three times)
 
For procedure details please look in the user manual positioned in LabManager.
=== RCA Cleaning of non-standard sample size ===
There are different possibilities in the RCA bench and in beakers in the fumehood. Please contact Nanolab staff in this situation.
 
'''The user manual, user APV and contact information can be found in LabManager:'''
<!-- remember to remove the type of documents that are not present -->
[http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=243 RCA info page in LabManager]


==Overview of RCA process data==
==Overview of RCA process data==


{| border="2" cellspacing="0" cellpadding="4" align="left" width="570pt"
{| border="2" cellspacing="0" cellpadding="4" align="left" width="570pt"
|-style="background:silver; color:black"
!  
!  
! RCA1
! RCA1 (SC-1)
! RCA2
! RCA2 (SC-2)
! HF
! HF
|-  
|-  
|-style="background:WhiteSmoke; color:black"
|'''General description'''
|'''General description'''
|
|
It is used for removal of light organics, particles and metal.
Used for removal of light organics, particles and desorption of trace metals (Au, Ag, Ni, Cd, Zn, Co, Cr, etc).
|
|
It is used for removal of heavy metals, alkalies and metal hydroxides.
Used for removal of alkali ions, metal hydroxides (of Al, Fe, Mg, Zn) and residual trace metals (e.g. Cu and Au).
|
|
It is used for removal of oxide generated in RCA1 and RCA2
Used for removal of oxide generated in RCA1 and RCA2
|-
|-
|-style="background:LightGrey; color:black"
|'''Chemical solution'''
|'''Chemical solution'''
|H<math>_2</math>O, NH<math>_4</math>OH(29%) and H<math>_2</math>O<math>_2</math>(30%) (5:1:1)
|H<sub>2</sub>O, NH<sub>4</sub>OH(25-29%) and H<sub>2</sub>O<sub>2</sub>(30%) (5:1:1)
|H<math>_2</math>O, HCl(37%) and H<math>_2</math>O<math>_2</math>(30%) (5:1:1)
|H<sub>2</sub>O, HCl(37%) and H<sub>2</sub>O<sub>2</sub>(30%) (5:1:1)
|5% HF
|5% HF
|-
|-
|-style="background:WhiteSmoke; color:black"
|'''Process temperature'''
|'''Process temperature'''
|70-80 <sup>o</sup>C
|70-80 <sup>o</sup>C
Line 45: Line 70:
|Room temperature  
|Room temperature  
|-
|-
|-style="background:LightGrey; color:black"
|'''Process time'''
|'''Process time'''
|
|
Line 53: Line 79:
30 sec.
30 sec.
|-
|-
|-style="background:WhiteSmoke; color:black"
|'''Life time of the chemical solutions'''
|'''Life time of the chemical solutions'''
|Can only be heated one time. When hot: it lasts for ~1h
|Can only be heated one time. When hot: it lasts for ~1h
Line 58: Line 85:
|~2 months
|~2 months
|-
|-
|-style="background:LightGrey; color:black"
|'''Allowed materials'''
|'''Allowed materials'''
|
|
Line 74: Line 102:
*Silicon nitride
*Silicon nitride
|-
|-
|-style="background:WhiteSmoke; color:black"
|'''Batch size'''
|'''Batch size'''
|
|
Line 82: Line 111:
1-25 2",4" or 6" wafers at a time
1-25 2",4" or 6" wafers at a time
|-
|-
|-style="background:LightGrey; color:black"
|'''Size of substrate'''
|'''Size of substrate'''
|
|
4"-6" wafers <br />
4"-6" wafers <br />
For 2" wafers please contact Danchip staff
For 2" wafers please contact Nanolab staff
|
|
4"-6" wafers <br />
4"-6" wafers <br />
For 2" wafers please contact Danchip staff
For 2" wafers please contact Nanolab staff
|
|
4"-6" wafers <br />
4"-6" wafers <br />
For 2" wafers please contact Danchip staff
For 2" wafers please contact Nanolab staff
|-
|-
|}
|}

Latest revision as of 08:24, 5 September 2025

The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.

Feedback to this page: click here

All links to Kemibrug (SDS) and Labmanager Including APV requires login.


RCA cleaning

RCA bench: positioned in cleanroom B1.
RCA1 - RCA2 - HF - BHF(pre-dep wafers)

The RCA cleaning procedure was originally developed by the Radio Corporation of America (RCA) as part of manufacturing electron tube components. This process has since been adapted to silicon semiconductor processing. RCA is a two-step process (RCA1 and RCA2, sometimes referred to as SC-1 and SC-2 (Standard Clean)), and RCA1 should always be made before RCA2 because removing organic contaminants is a requirement before metal contaminants can be removed effectively.

RCA1 is a powerful oxidizer and will thus remove organic contaminants. The ammonium hydroxide in RCA1 also has good solvating power as it can complex metals such as Cu, Ag, Ni, Co and Cd into solution. RCA2 forms soluble complexes with heavy metals and also shows cleaning action similar to that of piranha solutions. Furthermore, solutions of hydrochloric acid, which is a major constituent of RCA2, has proven effective at removing alkali metal ions. RCA2 is also effective at removing metal hydroxide traces that cannot be removed in ammonia-containing solutions such as RCA1. These include Al(OH)3, Fe(OH)3, Mg(OH)2 and Zn(OH)2. It is important that the chemicals used are very clean. RCA mixtures are therefore only used shortly after mixing and for a limited number of samples.

Since RCA1 can oxidize silicon to silicon dioxide, an HF dip is sometimes used between RCA1 and RCA2. This will also remove contaminants that can be trapped in the formed oxide. However, this step is often omitted, since RCA1 removes the native oxide and then re-oxidizes the surface. This in itself has a cleaning action. It is generally not advised to do an HF dip after RCA-2 if the samples will be processed by wet chemical processes afterwards. This is because the hydrogenated surface will be extremely reactive and therefore attract contaminants from both the air and processing liquids. In this case it is better to continue processing with the passivated oxide surface. RCA clean is often done prior to furnace processes, an in these cases an HF dip after RCA-2 makes sense. Ideally the wafers should be transferred to the furnace immediately after RCA cleaning, because the samples will be very sensitive to recontamination as mentioned above.

A crucial part of the RCA cleaning procedure is the oxidation by H2O2 at elevated temperatures. Therefore, the lifetime of RCA1 and RCA2 solutions is limited to about 1 hour after preparation and heating to 70oC because H2O2 decomposes at this temperature. A temperature of 70°C is optimal. RCA solutions should never be heated above 80°C since this will lead to excessive decomposition and loss of NH3.

  • RCA1 contains: H2O, NH4OH and H2O2 (5:1:1). It is used for removal of light organics, particles and metals.
  • RCA2 contains: H2O, HCl and H2O2 (5:1:1). It is used for removal of heavy metals, metal hydroxides, and residual metals including alkali metals.

You can find the APV for the RCA bench here

RCA procedure

  • RCA1: 10 min
  • DI water rinsing (dumping three times)
  • Optional: HF: 30 sec (you may avoid this step in case of a very thin oxide (0-200 Å) as the top layer)
  • DI water rinsing (bubbler)
  • RCA2: 10 min
  • DI water rinsing (dumping three times)
  • Optional: HF: 30 sec (avoid it if you have a very thin oxide (0-200 Å) as the top layer)
  • DI water rinsing (bubbler)

For procedure details please look in the user manual in LabManager.

RCA Cleaning of non-standard sample size

There are different possibilities in the RCA bench and in beakers in the fumehood. Please contact Nanolab staff in this situation.

The user manual, user APV and contact information can be found in LabManager: RCA info page in LabManager

Overview of RCA process data

RCA1 (SC-1) RCA2 (SC-2) HF
General description

Used for removal of light organics, particles and desorption of trace metals (Au, Ag, Ni, Cd, Zn, Co, Cr, etc).

Used for removal of alkali ions, metal hydroxides (of Al, Fe, Mg, Zn) and residual trace metals (e.g. Cu and Au).

Used for removal of oxide generated in RCA1 and RCA2

Chemical solution H2O, NH4OH(25-29%) and H2O2(30%) (5:1:1) H2O, HCl(37%) and H2O2(30%) (5:1:1) 5% HF
Process temperature 70-80 oC 70-80 oC Room temperature
Process time

10 min.

10 min.

30 sec.

Life time of the chemical solutions Can only be heated one time. When hot: it lasts for ~1h Can only be heated one time. When hot: it lasts for ~1h ~2 months
Allowed materials
  • Silicon
  • Silicon oxide
  • Silicon nitride
  • Quartz wafers/fused silica
  • Silicon
  • Silicon oxide
  • Silicon nitride
  • Quartz wafers/fused silica
  • Silicon
  • Silicon oxide
  • Silicon nitride
Batch size

1-25 2",4" or 6" wafers at a time

1-25 2",4" or 6" wafers at a time

1-25 2",4" or 6" wafers at a time

Size of substrate

4"-6" wafers
For 2" wafers please contact Nanolab staff

4"-6" wafers
For 2" wafers please contact Nanolab staff

4"-6" wafers
For 2" wafers please contact Nanolab staff