Jump to content

Specific Process Knowledge/Lithography/Strip: Difference between revisions

From LabAdviser
Jehem (talk | contribs)
Jehem (talk | contribs)
 
(122 intermediate revisions by the same user not shown)
Line 9: Line 9:


= Strip Comparison Table =
= Strip Comparison Table =
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"
{| class="wikitable"
 
|-
!colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment
!
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Strip#Plasma Asher 3: Descum|Plasma Asher 3: Descum]]</b>
! [[Specific_Process_Knowledge/Lithography/Strip/plasmaAsher03|Plasma Asher 3: Descum]]
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Strip#Plasma_Asher_4|Plasma Asher 4]]</b>
! [[Specific_Process_Knowledge/Lithography/Strip/plasmaAsher04|Plasma Asher 4 (Clean)]]
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Strip#Plasma Asher 5|Plasma Asher 5]]</b>
! [[Specific_Process_Knowledge/Lithography/Strip/plasmaAsher05|Plasma Asher 5 (Dirty)]]
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Strip#Resist Strip|Resist strip]]</b>
! [[Specific_Process_Knowledge/Lithography/Strip/resistStrip|Resist strip]]
|style="background:WhiteSmoke; color:black"|<b>[[Specific Process Knowledge/Lithography/LiftOff|Lift-off]]</b>
! [[Specific Process Knowledge/Lithography/LiftOff|Lift-off]]
 
|-
|-
!style="background:silver; width:100px; color:black;" align="center"|Purpose  
! scope=row style="text-align: left;" | Purpose  
|style="background:LightGrey; color:black"|
| Resist descum
|style="background:WhiteSmoke; color:black"|
|
Resist descum
*Resist stripping
|style="background:WhiteSmoke; color:black"|
*Resist descum
Clean wafers only, no metal
*Surface treatment
|style="background:WhiteSmoke; color:black"|
*Other ashing of organic material
All purposes
|
|style="background:WhiteSmoke; color:black"|
*Resist stripping
Resist strip, no metal lift off
*Resist descum
|style="background:WhiteSmoke; color:black"|
*Surface treatment
Lift-off
*Other ashing of organic material
 
| Resist stripping
| Metal lift-off
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="1"|Method
! scope=row style="text-align: left;" | Method
|style="background:LightGrey; color:black"|
| Plasma ashing
|style="background:WhiteSmoke; color:black"|
| Plasma ashing
Plasma ashing
| Plasma ashing
|style="background:WhiteSmoke; color:black"|
| Solvent & ultrasonication
Plasma ashing
| Solvent & ultrasonication
|style="background:WhiteSmoke; color:black"|
Plasma ashing
|style="background:WhiteSmoke; color:black"|
Solvent and ultra sound
|style="background:WhiteSmoke; color:black"|
Solvent and ultra sound
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameters
! scope=row style="text-align: left;" | Process gasses
|style="background:LightGrey; color:black"|Process gasses
| O<sub>2</sub> (50 sccm)
|style="background:WhiteSmoke; color:black"|
|
*O<sub>2</sub> (flow unknown)
|style="background:WhiteSmoke; color:black"|
*O<sub>2</sub> (0-500 sccm)
*O<sub>2</sub> (0-500 sccm)
*N<sub>2</sub> (0-500 sccm)
*N<sub>2</sub> (0-500 sccm)
|style="background:WhiteSmoke; color:black"|
|
*O<sub>2</sub> (0-500 sccm)
*O<sub>2</sub> (0-500 sccm)
*N<sub>2</sub> (0-500 sccm)
*N<sub>2</sub> (0-500 sccm)
*CF<sub>4</sub> (0-200 sccm)
*CF<sub>4</sub> (0-200 sccm)
|style="background:WhiteSmoke; color:black"|
| NA
*NA
| NA
|style="background:WhiteSmoke; color:black"|
|-
*NA
! scope=row style="text-align: left;" | Process power
 
| 10-100 W (10-100%)
| 150-1000 W
| 150-1000 W
| NA
| NA
|-
|-
|style="background:LightGrey; color:black"|Max. process power
! scope=row style="text-align: left;" | Process pressure
|style="background:WhiteSmoke; color:black"|
| 0.8 mbar
100 W (100%)
| 0.5-1.5 mbar<br>(standard process 1.3 mbar)
|style="background:WhiteSmoke; color:black"|
| 0.5-1.5 mbar<br>(standard process 1.3 mbar)
1000 W
| NA
|style="background:WhiteSmoke; color:black"|
| NA
1000 W
|style="background:WhiteSmoke; color:black"|
*NA
|style="background:WhiteSmoke; color:black"|
*NA
 
|-
|-
|style="background:LightGrey; color:black"|Solvent
! scope=row style="text-align: left;" | Process solvent
|style="background:WhiteSmoke; color:black"|
| NA
*NA
| NA
|style="background:WhiteSmoke; color:black"|
| NA
*NA
|
|style="background:WhiteSmoke; color:black"|
*NA
|style="background:WhiteSmoke; color:black"|
*NMP (Remover 1165)
*NMP (Remover 1165)
*Rinse in IPA
*IPA (rinsing agent)
|style="background:WhiteSmoke; color:black"|
|
*NMP (Remover 1165)
*NMP (Remover 1165)
*Rinse in IPA
*IPA (rinsing agent)
 
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
! scope=row style="text-align: left;" | Process temperature
|style="background:LightGrey; color:black"|Batch size
| Up to ~100°C
|style="background:WhiteSmoke; color:black"|
| Up to ~100°C
*1 small sample
| Up to ~100°C
*1 50 mm wafer
| Up to ~65°C
*1 100 mm wafer
| Up to ~65°C
|style="background:WhiteSmoke; color:black"|
*1 small sample
*1 50 mm wafer
*1-25 100 mm wafers
*1-25 150 mm wafers
*1-25 200 mm wafers
|style="background:WhiteSmoke; color:black"|
*1 small sample
*1 50 mm wafer
*1-25 100 mm wafers
*1-25 150 mm wafers
*1-25 200 mm wafers
|style="background:WhiteSmoke; color:black"|
*1 - 25 100 mm wafers
*1 - 25 150 mm wafers
|style="background:WhiteSmoke; color:black"|
*1 - 25 100 mm wafers
*1 - 25 150 mm wafers
|-
|-
|style="background:LightGrey; color:black"|Allowed materials
! scope=row style="text-align: left;" | Process time
|style="background:WhiteSmoke; color:black"|
| 1-10 minutes
*Silicon, glass, and polymer substrates
|  
*Film or pattern of all but Type IV
*Stripping: 20-90 minutes
|style="background:WhiteSmoke; color:black"|
*Descum: 5-15 minutes
*<b>No metals allowed - including metal oxides</b><br>
*Surface treatment: Seconds to minutes
*<b>No III-V materials</b>
*Other ashing: Hours, material dependent
*Silicon, glass, and polymer substrates
|  
*Film or pattern of photoresist/polymer
*Stripping: 20-90 minutes
|style="background:WhiteSmoke; color:black"|
*Descum: 5-15 minutes
*Silicon, III-V, and glass substrates
*Surface treatment: Seconds to minutes
*Film or pattern of all but Type IV
*Other ashing: Hours, material dependent
|style="background:WhiteSmoke; color:black"|
|
*<b>No metals allowed - including metal oxides</b><br>
*NMP (Remover 1165)
*Silicon, glass, and polymer substrates
*IPA (rinsing agent)
*Film or pattern of photoresist/polymer
|
|style="background:WhiteSmoke; color:black"|
*NMP (Remover 1165)
*Silicon and glass substrates
*IPA (rinsing agent)
*Film or pattern of all but Type IV
|-
|}
 
<br clear="all" />
 
= Plasma Ashing =
 
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"
|-
|-
 
! scope=row style="text-align: left;" | Substrate batch
|-style="background:silver; color:black"
|
*Chips: several
*50 mm wafer: several
*100 mm wafer: 1
|
*Chips: several
*50 mm wafer: several
*100 mm wafer: 1-25
*150 mm wafer: 1-25
*200 mm wafer: 1-25
|
*Chips: several
*50 mm wafer: several
*100 mm wafer: 1-25
*150 mm wafer: 1-25
*200 mm wafer: 1-25
|
*100 mm wafer: 1-25
*150 mm wafer: 1-25
|
|
! Photoresist stripping
*100 mm wafer: 1-25
! [[Specific_Process_Knowledge/Lithography/Descum|Descum after lithography]]
*150 mm wafer: 1-25
! Surface treatment of plastic, ceramic and metal
! Ashing of organic material
|-  
 
|-style="background:whitesmoke; color:black"
!Process pressure
|1.3 mbar
|1.3 mbar
|0.5-1.5 mbar
|0.5-1.5 mbar
|-
|-
 
! scope=row style="text-align: left;" | Substrate materials
|-style="background:silver; color:black"
|
!Process gases
*<span style="color:red">'''No polymer substrates'''</span><br>
*Silicon substrates
*III-V substrates
*Glass substrates
*Films, or patterned films, of any material except type IV (Pb, Te)
|
*<span style="color:red">'''No metals'''</span><br>
*<span style="color:red">'''No metal oxides'''</span><br>
*<span style="color:red">'''No III-V materials'''</span><br>
*Silicon substrates
*Glass substrates
*Polymer substrates
*Films, or patterned films, of resists/polymers
|
*Silicon substrates
*III-V substrates (only on Si carrier)
*Glass substrates
*Polymer substrates
*Films, or patterned films, of any material except type IV (Pb, Te)
|
|
*O<sub>2</sub> (100 sccm)
*<span style="color:red">'''No iron (Fe) containing films'''</span>
*N<sub>2</sub> (100 sccm)
*Silicon substrates
*III-V substrates
*Glass substrates
*Polymer substrates
*Films, or patterned films, of any material except type IV (Pb, Te)
|
|
*O<sub>2</sub> (100 sccm)
*<span style="color:red">'''No iron (Fe) or Copper (Cu) containing films'''</span>
*N<sub>2</sub> (100 sccm)
*Silicon substrates
|O<sub>2</sub>, CF<sub>4</sub>, N<sub>2</sub> or their mixtures
*III-V substrates (only if clean)
|O<sub>2</sub>
*Glass substrates
|-
*Films, or patterned films, of any material except type IV (Pb, Te)
 
|-style="background:whitesmoke; color:black"
!Process  power
|1000 W
|200 W
|150-1000 W
|1000 W or less for heat- sensitive materials
|-
 
|-style="background:silver; color:black"
!Process  time
|5-90 minutes
|1-30 minutes
|seconds to minutes
|Between 0.5 and 20 hours, depending on the material
|-
 
|-style="background:whitesmoke; color:black"
!Batch size
|1-25
|1-25
|1 wafer at a time
|1 wafer at a time, use a container, e.g Petri dish
|-
|}
|}


<br clear="all" />
=Decommisioned tools=
 
<!--
Typical process time for stripping in plasma asher 1 or 2:
*1.5 µm AZ 5214E resist film: ~15 min
*10 µm AZ 4562 resist film: ~45 min
 
Typical process parameters:
*O<sub>2</sub>: 400 ml/min
*N<sub>2</sub>: 70 ml/min
*Power: 1000 W
 
 
A typical descum process in plasma asher 1 or 2:
*O<sub>2</sub>: 70 ml/min
*N<sub>2</sub>: 70 ml/min
*Power: 150 W
*Time : 10 min
 
 
Be sure to wait for chamber to cool down to room temperature, before runinng descum processes in plasma asher 1 or 2. At a load of 2 Fused silica wafers, the amount of resist removed will be 10 - 1500 nm.
 
'''NB: Use dedicated descum asher Plasma Asher 3: Descum for descumming.'''
-->
 
==Process gas ratio for plasma asher 4 & 5==
[[File:PA_gas_mix_v3.png|320px|thumb|Ashing rate as function of gas mix ratio when processing a single 100 mm wafer and when processing a full boat with 25 wafers.|right]]
The ashing rate is related to the gas mix, usually expressed as percentage of nitrogen of the total amount of gas.
 
Testing found that a gas mix of 50% nitrogen gives the highest ashing rate for both processing single substrates and when processing a full boat with 25 substrates. Please note that the ashing rate for a full boat is approximately ten times slower, than when processing a single substrate.
 
'''Single substrate:'''<br>
Test using a single 100 mm wafer in the center of the process chamber shows that 30-80% nitrogen gives the highest ashing rate.
 
Total gas flow rate: 500 sccm<br>
Gas mix ratio: tested parameter<br>
Chamber pressure: 1.25 mbar<br>
Power: 1000 W<br>
Processing time: 2 minutes<br>
Temperature (average): 43°C
<br clear="all" />
 
'''Full boat:'''<br>
Test using a boat of 25 100 mm wafers in the center of the process chamber shows that 50-70% nitrogen gives the highest ashing rate.
 
Total gas flow rate: 200 sccm<br>
Gas mix ratio: tested parameter<br>
Chamber pressure: 1.3 mbar<br>
Power: 1000 W<br>
Processing time: 10 minutes<br>
Temperature (average): 43°C
<br clear="all" />
 
==Process chamber pressure for plasma asher 4 & 5==
[[File:PA_chamber_pressure_v3.png|320px|thumb|Ashing rate as function of chamber pressure when processing a single substrate and when processing a full boat with 25 substrates.|right]]
The ashing rate is related to the chamber pressure during processing.
 
Testing found that 1.3 mbar gives the highest ashing rate for both processing single substrates and when processing a full boat with 25 substrates. Please note that the ashing rate for a full boat is approximately ten times slower, than when processing a single substrate.
 
'''Single substrate:'''<br>
Test using a single 100 mm wafer in the center of the process chamber shows that 1.3 mbar gives the highest ashing rate.
 
Total gas flow rate: 500 sccm<br>
Gas mix ratio: 30% nitrogen<br>
Chamber pressure: tested parameter<br>
Power: 1000 W<br>
Processing time: 2 minutes<br>
Temperature (average): 43°C
<br clear="all" />
 
'''Full boat:'''<br>
Test using a boat of 25 100 mm wafers in the center of the process chamber shows that 1.4 mbar gives the highest ashing rate.
 
Total gas flow rate: 200 sccm<br>
Gas mix ratio: 30% nitrogen<br>
Chamber pressure: tested parameter<br>
Power: 1000 W<br>
Processing time: 10 minutes<br>
Temperature (average): 43°C
<br clear="all" />
 
==Process gas flow rate for plasma asher 4 & 5==
[[File:PA_flowRate_v4.png|320px|thumb|Ashing rate as function of total gas flow when processing a single substrate and when processing a full boat with 25 wafers.|right]]
The ashing rate is related to the total gas flow rate during processing.
 
Testing found that 200 sccm gives the highest ashing rate for both processing single substrates and when processing a full boat with 25 substrates. Please note that the ashing rate for a full boat is approximately ten times slower, than when processing a single substrate.
 
'''Single substrate:'''<br>
Test using a single 100 mm wafer in the center of the process chamber shows that 200 sccm gives the highest ashing rate.
 
Total gas flow rate: tested parameter<br>
Gas mix ratio: 30% nitrogen<br>
Chamber pressure: 1.3 mbar<br>
Power: 1000 W<br>
Processing time: 2 minutes<br>
Temperature (average): 43°C
<br clear="all" />
 
'''Full boat:'''<br>
Test using a boat of 25 100 mm wafers in the center of the process chamber shows that 200 sccm gives the highest ashing rate.
 
Total gas flow rate: tested parameter<br>
Gas mix ratio: 30% nitrogen<br>
Chamber pressure: 1.3 mbar<br>
Power: 1000 W<br>
Processing time: 10 minutes<br>
Temperature (average): 43°C
<br clear="all" />
 
==Process power for plasma asher 4 & 5==
[[File:PA_power_v2.png|320px|thumb|Ashing rate as function of microwave power.|right]]
The ashing rate is related to the power used during processing. Higher power gives higher ashing rate.
 
'''Single substrate:'''<br>
Test using a single 100 mm wafer in the center of the process chamber shows that a power of 1000 W gives the highest ashing rate.
 
Total gas flow rate: 200 sccm<br>
Gas mix ratio: 30% nitrogen<br>
Chamber pressure: 1.3 mbar<br>
Power: tested parameter<br>
Processing time: 2 minutes<br>
Temperature (average): 43°C
<br clear="all" />
 
==Process temperature for plasma asher 4 & 5==
[[File:PA_temperature_v1.png|320px|thumb|Ashing rate as function of temperature.|right]]
The ashing rate is related to the temperature during processing. Higher temperature gives higher ashing rate.
 
'''Single substrate:'''<br>
Test using a single 100 mm wafer in the center of the process chamber shows that increasing processing temperature gives increasing ashing rate.
 
Total gas flow rate: 200 sccm<br>
Gas mix ratio: 30% nitrogen<br>
Chamber pressure: 1.3 mbar<br>
Power: 1000 W<br>
Processing time: 2 minutes<br>
Temperature (average): tested parameter
<br clear="all" />
 
=Plasma Asher 1=
<span style="color:red">Plasma asher 1 was decommissioned 2024-12-02.</span>
<span style="color:red">Plasma asher 1 was decommissioned 2024-12-02.</span>


[[Specific Process Knowledge/Lithography/Strip/PlasmaAsher1|Information about decommissioned tool can be found here.]]
[[Specific Process Knowledge/Lithography/Strip/PlasmaAsher1|Information about decommissioned tool can be found here.]]


=Plasma Asher 2=
 
<span style="color:red">Plasma asher 2 was decommissioned 2024-12-02.</span>
<span style="color:red">Plasma asher 2 was decommissioned 2024-12-02.</span>


[[Specific Process Knowledge/Lithography/Strip/PlasmaAsher2|Information about decommissioned tool can be found here.]]
[[Specific Process Knowledge/Lithography/Strip/PlasmaAsher2|Information about decommissioned tool can be found here.]]
=Plasma Asher 3: Descum=
[[image:2017-03-15 13.12.45.jpg|350x350px|thumb|Plasma Asher 3: Descum is placed A-5]]
The Plasma Asher 3: Descum dedicated for resist descum i.e. removal of remains resist traces after development. It has a small chamber, so you can only load a single 100 mm substrate or a few smaller pieces.
In this machine, only O2 and N2 gases are used for processes.
<b>Typical process parameters when operating the equipment:</b><br>
Process: Photoresist descum<br>
Pressure: 0.2-0.8 mbar<br>
Gas: O<sub>2</sub><br>
Power: 50-100%<br>
Time:1 -10 minutes (depending on photoresist type and thickness)<br>
The other materials have not been tested yet.
The user manual, user APV, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=423 LabManager] - '''requires login'''
===Process Information===
Detailed information about descum processing on Plasma asher 3: Descum can be found [[Specific Process Knowledge/Lithography/Descum|here]].
<br clear="all" />
<!-- TARAN 220-03-05
==III-V Plasma Asher==
[[Image:III-V_asher.jpg|300x300px|thumb|Plasma asher for removing resist on III-V samples: positioned in A-5]]
Diener Pico Plasma Asher for III-V materials.
The user manual and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=186 LabManager] - '''requires login'''
<br clear="all" />
<br clear="all" />
-->
=Plasma Asher 4=
[[File:PA5 front.jpg|320px|thumb|Plasma asher 4 in cleanroom E-5.|right]]
The Plasma Asher 4 can be used for the following processes:
*Photoresist stripping
*Descumming
*Surface cleaning
*Removal of organic passivation layers and masks
Plasma asher 4 has the following material restrictions:
*No metals allowed
*No metal oxides allowed
*No III-V materials allowed
The user manual, risk assessment, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=530 LabManager] - '''requires login'''
===Process Information===
*[[Specific Process Knowledge/Lithography/Descum#Plasma Asher 4|Descum using plasma asher 4]]
'''Typical stripping parameters'''
*Resist: 1.5 µm AZ 5214E
*Substrate: 100 mm Si
*O<sub>2</sub>: 100 sccm
*N<sub>2</sub>: 100 sccm
*Pressure (DSC): 1.3 mbar
*Power: 1000 W
*Time (single wafer): 20 minutes
*Time (full boat): 90 minutes
The user manual, user APV, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=200 LabManager] - '''requires login'''
===Process Information===
*[[Specific Process Knowledge/Lithography/Descum|Descum]]
<br clear="all" />
=Plasma Asher 5=
[[File:PA5 front.jpg|320px|thumb|Plasma asher 5 in cleanroom E-5.|right]]
The Plasma Asher 5 can be used for the following processes:
*Photoresist stripping
*Descumming
*Surface cleaning
*Removal of organic passivation layers and masks
Furthermore plasma processing using CF<sub>4</sub> in plasma asher 5 can be used for:
*Etching of glass and ceramic
*Etching of SiO<sub>2</sub>, Si<sub>3</sub>N<sub>4</sub>, Si
*Removal of polyimide layers
'''Typical stripping parameters'''
*Resist: 1.5 µm AZ 5214E
*Substrate: 100 mm Si
*O<sub>2</sub>: 100 sccm
*N<sub>2</sub>: 100 sccm
*Pressure (DSC): 1.3 mbar
*Power: 1000 W
*Time (single wafer): 20 minutes
*Time (full boat): 90 minutes
Plasma asher 5 can be used for almost every material, but if you have any doubt if your materials are compatible/allowed in plasma asher 5, feel free to ask the lithography group at Nanolab.
The user manual, risk assessment, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=531 LabManager] - '''requires login'''
===Process Information===
*[[Specific Process Knowledge/Etch/Etching of Silicon Oxide/SiO2 etch using Plasma Asher |SiO<sub>2</sub> etch using Plasma Asher 5]]
*[[Specific Process Knowledge/Lithography/Descum#Plasma Asher 5|Descum using plasma asher 5]]
<br clear="all" />
=Resist Strip=
[[Image:Resist_strip.jpg|300x300px|thumb|Resist strip bench in D-3]]
This resist strip is only for wafers without metal and SU-8.
There are one Remover 1165 bath for stripping and one IPA bath for rinsing.
'''Here are the main rules for resist strip use:'''
*Place the wafers in a wafer holder and put them in the first bath for 10 min, this time is depending how much resist you have on the surface.
*After the strip rinse your wafers in the IPA bath for 2-3 min.
*Rinse your wafers for 4-5 min. in running water after stripping.
The user manual and contact information can be found in LabManager: [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=385 Resist Strip] - '''requires login'''
<br clear="all" />
==Overview of wet bench 06 and 07==
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"
|-style="background:silver; color:black"
|
! [[Specific Process Knowledge/Lithography/Strip#Resist_Strip|Resist Strip]]
! [[Specific Process Knowledge/Lithography/LiftOff#Lift-off_wet_bench_07|Lift-off]]
|-
|-style="background:whitesmoke; color:black"
!General description'''
|Wet stripping of resist
|Lift-off process
|-
|-style="background:silver; color:black"
!Chemical solution
|NMP Remover 1165
|NMP Remover 1165
|-
|-style="background:whitesmoke; color:black"
!Process temperature
|Up to 65°C
|Up to 65°C
|-
|-style="background:silver; color:black"
!Batch size
|
1 - 25 wafers
|
1 - 25 wafers
|-
|-style="background:whitesmoke; color:black"
!Size of substrate
|
*100 mm wafers
*150 mm wafers
|
*100 mm wafers
*150 mm wafers
|-
|-style="background:silver; color:black"
!Allowed materials
|
*Silicon
*Silicon Oxide
*Silicon Nitride
*Silicon Oxynitride
|
All metals except Type IV (Pb, Te)
|-
|}

Latest revision as of 08:57, 21 September 2026

The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.

Feedback to this page: click here

Strip Comparison Table

Plasma Asher 3: Descum Plasma Asher 4 (Clean) Plasma Asher 5 (Dirty) Resist strip Lift-off
Purpose Resist descum
  • Resist stripping
  • Resist descum
  • Surface treatment
  • Other ashing of organic material
  • Resist stripping
  • Resist descum
  • Surface treatment
  • Other ashing of organic material
Resist stripping Metal lift-off
Method Plasma ashing Plasma ashing Plasma ashing Solvent & ultrasonication Solvent & ultrasonication
Process gasses O2 (50 sccm)
  • O2 (0-500 sccm)
  • N2 (0-500 sccm)
  • O2 (0-500 sccm)
  • N2 (0-500 sccm)
  • CF4 (0-200 sccm)
NA NA
Process power 10-100 W (10-100%) 150-1000 W 150-1000 W NA NA
Process pressure 0.8 mbar 0.5-1.5 mbar
(standard process 1.3 mbar)
0.5-1.5 mbar
(standard process 1.3 mbar)
NA NA
Process solvent NA NA NA
  • NMP (Remover 1165)
  • IPA (rinsing agent)
  • NMP (Remover 1165)
  • IPA (rinsing agent)
Process temperature Up to ~100°C Up to ~100°C Up to ~100°C Up to ~65°C Up to ~65°C
Process time 1-10 minutes
  • Stripping: 20-90 minutes
  • Descum: 5-15 minutes
  • Surface treatment: Seconds to minutes
  • Other ashing: Hours, material dependent
  • Stripping: 20-90 minutes
  • Descum: 5-15 minutes
  • Surface treatment: Seconds to minutes
  • Other ashing: Hours, material dependent
  • NMP (Remover 1165)
  • IPA (rinsing agent)
  • NMP (Remover 1165)
  • IPA (rinsing agent)
Substrate batch
  • Chips: several
  • 50 mm wafer: several
  • 100 mm wafer: 1
  • Chips: several
  • 50 mm wafer: several
  • 100 mm wafer: 1-25
  • 150 mm wafer: 1-25
  • 200 mm wafer: 1-25
  • Chips: several
  • 50 mm wafer: several
  • 100 mm wafer: 1-25
  • 150 mm wafer: 1-25
  • 200 mm wafer: 1-25
  • 100 mm wafer: 1-25
  • 150 mm wafer: 1-25
  • 100 mm wafer: 1-25
  • 150 mm wafer: 1-25
Substrate materials
  • No polymer substrates
  • Silicon substrates
  • III-V substrates
  • Glass substrates
  • Films, or patterned films, of any material except type IV (Pb, Te)
  • No metals
  • No metal oxides
  • No III-V materials
  • Silicon substrates
  • Glass substrates
  • Polymer substrates
  • Films, or patterned films, of resists/polymers
  • Silicon substrates
  • III-V substrates (only on Si carrier)
  • Glass substrates
  • Polymer substrates
  • Films, or patterned films, of any material except type IV (Pb, Te)
  • No iron (Fe) containing films
  • Silicon substrates
  • III-V substrates
  • Glass substrates
  • Polymer substrates
  • Films, or patterned films, of any material except type IV (Pb, Te)
  • No iron (Fe) or Copper (Cu) containing films
  • Silicon substrates
  • III-V substrates (only if clean)
  • Glass substrates
  • Films, or patterned films, of any material except type IV (Pb, Te)

Decommisioned tools

Plasma asher 1 was decommissioned 2024-12-02.

Information about decommissioned tool can be found here.


Plasma asher 2 was decommissioned 2024-12-02.