Jump to content

Specific Process Knowledge/Characterization/Profiler: Difference between revisions

From LabAdviser
Reet (talk | contribs)
Mmat (talk | contribs)
mNo edit summary
 
(76 intermediate revisions by 4 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:Characterization@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Characterization/Profiler click here]'''
to be deleted, info copied to pages with respective tool name


[[Category: Equipment|Characterization Profiler]]
https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Characterization/Dektak_XTA
[[Category: Characterization|Profiler]]


https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Characterization/Tencor_P17


==Overview of the Nanolab profilers==
https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Characterization/Sensofar_S_Neox
All the profilers are compared on the [[Specific Process Knowledge/Characterization/Topographic measurement#Comparison_of_stylus_profilers.2C_optical_profilers_and_AFMs_at_Nanolab|topographic measurement]] page.


The sections below describe each profiler (stylus profilers and optical profilers) in more detail.
https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Characterization/Filmetrics


==Dektak XTA stylus profiler==
https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Characterization/Dektak_3ST


The Dektak XTA stylus profiler from Brüker is used for profiling surfaces of samples with structures in the micro- and nanometer range. The size of the structures that can be measured is limited by the tip dimensions.
https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Characterization/Dektak_150
 
A profile measurement can be done across a specific structure by using a high magnification camera to locate the structure. It is also possible to program the stylus to measure in several positions, defined with respect to some deskew points. [[Specific_Process_Knowledge/Characterization/Stress_measurement|Stress measurements]] of thin films can be done by measuring the wafer bow.
 
 
'''The user manual, quality control procedure and results, technical information and contact information can be found in LabManager:'''
 
[http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=304 Dektak XTA in LabManager]
 
 
===Equipment performance and process related parameters===
 
[[image:Dektak XTA new.JPG|275x275px|right|thumb|Dektak XTA: positioned in cleanroom F-2.]]
 
{| border="2" cellspacing="0" cellpadding="10"
|-
!style="background:silver; color:black;" align="left"|Purpose
|style="background:LightGrey; color:black"|Profiler for measuring micro structures||style="background:WhiteSmoke; color:black"|
*Single line profiles
*Wafer mapping
*[[Specific_Process_Knowledge/Characterization/Stress_measurement|Stress measurements]] by measuring wafer bow
*Surface roughness on a line scan
|-
!style="background:silver; color:black" align="left" rowspan="6" valign="top" |Performance
|style="background:LightGrey; color:black"|Scan range x y
|style="background:WhiteSmoke; color:black"|
Line scan x: 50 µm to 55 mm in a single scan, up to 200 mm with stiching
|-
|style="background:LightGrey; color:black"|Scan range z
|style="background:WhiteSmoke; color:black"|
50 Å to 1 mm
|-
|style="background:LightGrey; color:black"|Resolution x y
|style="background:WhiteSmoke; color:black"|
Down to 0.003 µm
|-
|style="background:LightGrey; color:black"|Resolution z
|style="background:WhiteSmoke; color:black"|
1 Å, 10 Å, 80 Å or 160 Å (for ranges 65 kÅ, 655 kÅ, 5240 kÅ and 1 mm respectively)
|-
|style="background:LightGrey; color:black"|Height accuracy z (95 % confidence)
|style="background:WhiteSmoke; color:black"|
~ 18 nm for the 65 kÅ range; ~ 0.17 µm for the intermediate ranges, and ~0.22 µm for the 1 mm range '''for well-defined steps that are easy to measure reproducibly''' ([[#Height measurement accuracy for the DektakXT|see below]])
|-
|style="background:LightGrey; color:black"|Max scan depth as a function of trench width W
|style="background:WhiteSmoke; color:black"|
1.2*(W[µm]-5µm)
 
|-
!style="background:silver; color:black" align="left"|Hardware settings
|style="background:LightGrey; color:black"|Tip radius
|style="background:WhiteSmoke; color:black"|
*5 µm 45<sup>o</sup> cone
|-
!style="background:silver; color:black" align="left" rowspan="5" valign="top" |Substrates
|style="background:LightGrey; color:black"|Substrate size
|style="background:WhiteSmoke; color:black"|
*Up to 6"
|-
| style="background:LightGrey; color:black"|Substrate materials allowed
|style="background:WhiteSmoke; color:black"|
*In principle all materials
|-
|}
 
===Height measurement accuracy===
The accuracy of a height measurement with the profiler depends on the measurement settings, the sample, the instrument calibration and the resolution.
 
====Use the right measurement settings for your sample====
Both the force setting and the scan speed are important: Too high force may compress a soft material like Al, Au or some polymers, while too low force may lead to the stylus "jumping" over features, especially if the scan speed is high.
 
If the scan speed is too low and you are measuring a small step <500 nm, you may experience drift in the measurement. Of course you also must make sure the feature you are measuring is wide enough and the scan speed is low enough for the stylus tip to reach the bottom of the feature (see the [http://labmanager.dtu.dk/d4Show.php?id=2346&mach=304 DektakXT manual], Figure 3 for details).
 
A sharp vertical step is easiest to measure. If the step is gradual or the surface is very rough, it can be difficult to determine where to measure and how the scan should be leveled.
 
====Influence of calibration standard uncertainty====
Nanolab staff check the instrument's measurement accuracy with a standard step height of 917 nm for the 65 kÅ range and 24.925 µm for the larger ranges. The 95 % confidence intervals for the standards are 17 nm for the 9160 Å standard and 0.072 µm for the 24.925 µm standard. If the control measurement is beyond the limit set in our Quality Control procedure, the instrument is calibrated and the users informed (see LabManager for details on the [http://labmanager.dtu.dk/d4Show.php?id=2493&mach=304 control instruction] and the [https://labmanager.dtu.dk/view_binary.php?type=data&mach=304 control measurement data]).
 
The size of the calibration standard confidence intervals mean that the measurement uncertainty is much more significant for very shallow steps below 500 nm than for steps in the micron range: The 95 % confidence interval of a 1 µm step measured with the 65 kÅ range is at least the ± 17 nm error of the standard step, so measuring a 100 nm step will have a similar error percentage-wise. Note that this error (from the calibration standard) is systematic. The random error associated with repeated measurements can be smaller for rigid, well defined vertical steps (perhaps ± 5 nm). One can therefore measure shallow steps to compare samples even if the absolute numbers are not totally reliable.
 
====Total uncertainty====
[[File:Error probability distributions sep 2020 update big.png|upright=2|alt=Four different probability distributions that contribute to the total error on the Dektak measurement for the 6.5 micron range. By far the widest distribution is the one from the error on the calibration standard, which is a Gaussian. The others are the non-Gaussian spread of the average measurement of the calibration standard height, which cuts off at the QC limits, the resolution, which is a very narrow uniform distribution, and the spread of measurement values for a given step being measured, which is a Gaussian whose width depends on the step in question.|right|thumb|The probability distributions of the main sources of error that are convoluted to create the total error on a Dektak measurement.]]
 
To estimate the accuracy of the Dektak's measurements we have to combine the error of the calibration with the error from the limit on the resolution and the scatter of repeated measurements. This is shown graphically on the right. You can see an uncertainty budget for the Dektak measurements here (made by Rebecca Ettlinger): [[Media:uncertainty budget Dektak.xlsx]]. It is based on the assumption that all the error sources are independent and can therefore be added by the sum of squares method, which you can read about here: [[Media:JCGM_100_2008_E.pdf]].
 
The error stemming from the uncertainty on the calibration standard dominates for the 6.5 micron range, while for the other ranges the scatter of repeated measurements is also important. Using the sum of squares method leads to the 95 % confidence intervals listed above in the table: just over 18 nm for the smallest range and around 0.2 µm for the other ranges.
 
As noted above, be aware that if you have a step height that is difficult to measure, the scatter of repeated measurements could easily lead to larger confidence intervals. To improve the accuracy of your particular measurement, you should repeat the measurement several times and estimate the standard deviation. If the scatter of your measurements is large, you can use our uncertainty budget to calculate the cumulative uncertainty for your own sample.
 
<br clear="all" />
 
==Stylus Profiler (Tencor P17) ==
 
The P17 Stylus Profiler from KLA Tencor is used in a similar manner to the Dektak XTA for profiling surfaces with structures in the micro- and submicrometer range as well as stress mapping and roughness measurements. It has more advanced options for [[Specific_Process_Knowledge/Characterization/Stress_measurement|stress measurements]] than the Dektak XTA and allows the user to measure a stress map with down to 5° radial resolution.
 
A line profile may be done across a specific structure located with a camera. It is also possible to measure many parallel scans to map out a surface, or to program a sequence of scans in different locations on a wafer defined with respect to some deskew points. Programming a sequence is somewhat easier and the manual for doing it much better for the P17 than for the Dektak XTA.
 
A disadvantage of the P17 is that is can be hard to locate the structures one wants to measure as the maximum field of view of the camera is 1x1.5 mm. We recommend knowing your sample well or having a picture of the sample design available so you can easily locate the features of interest. Otherwise the P17 is easy to use, fast and accurate, just like the DektakXT.
 
'''The user manual, quality control procedure and results, technical information and contact information can be found in LabManager:'''
 
[http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=486 P17 page in LabManager]
 
 
'''Info about using the analysis software from outside the cleanroom:'''
[[Specific_Process_Knowledge/Characterization/Profiler/Apex software|Apex software access]]
 
===Equipment performance and process related parameters===
 
[[image:KLA-Tencor P17 profiler.jpg|275x275px|right|thumb|Front of the P17 profiler located in cleanroom F-2.]]
 
{| border="2" cellspacing="0" cellpadding="10"
|-
!style="background:silver; color:black;" align="left"|Purpose
|style="background:LightGrey; color:black"|Profiler for measuring microstructures||style="background:WhiteSmoke; color:black"|
*Single line profiles
*Wafer mapping
*[[Specific_Process_Knowledge/Characterization/Stress_measurement|Stress measurements]] by measuring the wafer bow
*Surface roughness on a line scan
|-
!style="background:silver; color:black" align="left" rowspan="6" valign="top" |Performance
|style="background:LightGrey; color:black"|Scan range X Y
|style="background:WhiteSmoke; color:black"|
Line scan X: 20 µm to 200 mm in a single scan. No stitching.
 
Map scan XY: any rectangle that can be inscribed in a 200 mm circle. Note limited resolution (max. 4 million points). Scanning a large area accurately will be slow.
|-
|style="background:LightGrey; color:black"|Scan range Z
|style="background:WhiteSmoke; color:black"|
50 nm to 900 µm (it is possible to measure smaller steps but not recommended as the results may not be accurate)
|-
|style="background:LightGrey; color:black"|Resolution X Y
|style="background:WhiteSmoke; color:black"|
Down to 0.025 µm
|-
|style="background:LightGrey; color:black"|Resolution Z
|style="background:WhiteSmoke; color:black"|
0.01 Å, 0.08 Å, or 0.6 Å according to the manufacturer for ranges 13 µm, 131 µm, and 1 mm.†
|-
|style="background:LightGrey; color:black"|Height accuracy z (95 % confidence)
|style="background:WhiteSmoke; color:black"|
On the order of 17 nm for the smallest range for a 1 micron step and 0.2 micron for the larger ranges for a 25 micron step '''for well-defined steps that are easy to measure''', see section above.
|-
|style="background:LightGrey; color:black"|Max scan depth as a function of trench width W
|style="background:WhiteSmoke; color:black"|
0.87*(W[µm]-2µm) = tan(60<sup>o</sup>)/2*(W[µm]-2µm)
(empirically validated by Nanolab staff)
|-
!style="background:silver; color:black" align="left"|Hardware settings
|style="background:LightGrey; color:black"|Tip radius
|style="background:WhiteSmoke; color:black"|
*2 µm 60<sup>o</sup> cone
|-
!style="background:silver; color:black" align="left" rowspan="5" valign="top" |Substrates
|style="background:LightGrey; color:black"|Substrate size
|style="background:WhiteSmoke; color:black"|
*Up to 8"
|-
| style="background:LightGrey; color:black"|Substrate materials allowed
|style="background:WhiteSmoke; color:black"|
*In principle all materials that do not leave residues on the chuck.
|-
|}
 
†The resolution for the smallest range is theoretical, as this is below the noise threshold at least in our lab.
 
===Height measurement accuracy for the Tencor P17 Stylus Profiler===
This is similar to what applies to the DektakXT as described above. The P17 has slightly better reproducibility but as the uncertainty for small steps is dominated by the uncertainty on the standard step height's actual size, this does not make much difference. For the larger ranges the uncertainty is similar to that of the intermediate ranges of the DektakXT. Note that just as for the Dektak, the reproducibility of your own measurements of your particular step can make a relatively large contribution to the total uncertainty, Steps in real devices are not always as easy to measure or as well defined as our standard step height measurements.
<br clear="all" />
 
==Optical Profiler (Sensofar S Neox) ==
 
[[image:IMG_4555.JPG|275x275px|right|thumb|Optical Profiler (Sensofar): positioned in the clean room C-1)]]
 
The Sensofar S Neox 3D Optical Profiler has a sensor head that combines confocal, interferometry and focus variation techniques  as well as thick and thin film measurement capabilities.
 
The Neox sensor head provides standard microscope imaging, confocal imaging, confocal profiling, PSI (Phase Shift Interferometry), CSI (Coherence Scanning Interferometry), Active illumination (Ai) Focus Variation and high resolution thin film thickness measurements on a single instrument.
 
The main purpose is 3D topographic imaging of surfaces, step height measurements in smaller trenches/holes than can be obtained with standard stylus methods (i.e. with aspect ratios higher that 1:1), roughness measurements with larger FOV (Field Of View) than the AFM, but less horisontal resolution.
 
For most samples the optical profiler provides fast and easy information without any sample preparation. However, it can be necessary to cover thin transparent layers (< 2 µm) with a thin layer of metal.
 
The resolution is limited by the objectives and the pixel resolution.
[[Image:3D examples.JPG|200px|right]]
 
'''Analysis software:'''
*Free analysis software for visualizing and analyzing AFM and Optical profiler files (Sensofar) [http://gwyddion.net Gwyddion]
*SensoView software from Sensfar want also be downloaded for all users: U:\Nlab\CleanroomDrive\_Equipment\Optical profiler Sensofar\SensoVIEW 1.6.0
 
 
'''The user manual, technical information (SensoSCAN and SensoVIEW manuals) and contact information can be found in LabManager:'''
 
[http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=491 Optical profiler (Sensofar S Neox) info page in LabManager]
 
 
===Process Information===
 
*[[Media:Plu neox 2010.pdf| Sensofar presentation on how the sensofar works (for the previous system but the techniques are the same)]]
*[[Media:BR90-05F-EN-Brochure-S-neox.pdf|S Neox leaflet including specifications]]
*[[/Optical Profiler (Sensofar) acceptance test|Results from the Optical Profiler (Sensofar) acceptance test - for the previous system - expired!!]]
*Acceptance measurements on the S Neox Sensofar: [[Media:Acceptance measurements on Nanolab samples.pdf]]
 
===Equipment performance and process related parameters===
 
{| border="2" cellspacing="0" cellpadding="10"
 
!colspan="2" border="none" style="background:silver; color:black;" align="center"|<b>Equipment</b>
|style="background:WhiteSmoke; color:black"|<b>Optical profiler</b>
|-
!style="background:silver; color:black;" align="left"|Purpose
|style="background:LightGrey; color:black"|3D topographic imaging of surfaces.||style="background:WhiteSmoke; color:black"|
*3D imaging of surfaces
*Roughness measurements
*Step height measurements
*3D topographic measurements
*Thick and thin film thickness measurements in small spots
|-
!style="background:silver; color:black;" align="left"|Posibilities
|style="background:LightGrey; color:black"|Confocal, interferometric and AI focus variation tophography and reflectometry
*Standard microscope imaging
*Confocal imaging
*Confocal profiling
*PSI (Phase Shift Interferometry)
*CSI (Coherence Scanning Interferometry)
*Active illumination (Ai) Focus Variation
*High resolution thin film thickness measurement using reflectrometry
*Stitched scans
*Wafer mapping
|style="background:WhiteSmoke; color:black"|
 
[[image:Techniques overview.JPG]]
|-
!style="background:silver; color:black" align="left"|Performance
|style="background:LightGrey; color:black"|Depending on the objective chosen||style="background:WhiteSmoke; color:black"|
*See the performance of the different objectives here:
[[image:Objectives01.JPG|600px|Objectives01.JPG]]
|-
|-
!style="background:silver; color:black" align="left"|Substrates
|style="background:LightGrey; color:black"|Substrate size
|style="background:WhiteSmoke; color:black"|
*Substrates no bigger than 150 mm x 150mm
|-
|style="background:silver; color:black"|
| style="background:LightGrey; color:black"|Substrate materials allowed
|style="background:WhiteSmoke; color:black"|
*In principle all materials as long as they are allowed in the cleanroom outside fumehoods - no liquids!
|-
|}
 
==Optical Profiler (Filmetrics)==
 
[[image:Scanner without anotation.jpg|275x275px|right|thumb|Optical Profiler (Filmetrics): positioned in the basement (346-904)]]
 
The Profilm3D optical profiler from Filmetrics uses white-light-interferometry (WLI) and phase-shifting-interferometry (PSI) to produce surface profiles and depth-of-field color images.
 
The main purpose is 3D topographic imaging of surfaces, step height measurements and roughness measurements with larger FOV (Field Of View) than the AFM, but less horisontal resolution.
 
For most samples the optical profiler provides fast and easy information without any sample preparation. However, it can be necessary to cover thin transparent layers (< 2 µm) with a thin layer of metal.
 
The resolution is limited by the objective and the sampling resolution.
 
 
'''The user manual, technical information and contact information can be found in LabManager:'''
 
[http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=467 Optical profiler (Filmetrics) info page in LabManager]
 
 
 
===Equipment performance and process related parameters===
 
{| border="2" cellspacing="0" cellpadding="10"
 
!colspan="2" border="none" style="background:silver; color:black;" align="center"|<b>Equipment</b>
|style="background:WhiteSmoke; color:black"|<b>Optical profiler</b>
|-
!style="background:silver; color:black;" align="left"|Purpose
|style="background:LightGrey; color:black"|3D topographic imaging of surfaces.||style="background:WhiteSmoke; color:black"|
*3D imaging of surfaces
*Roughness measurements
*Step height measurements
*3D topographic measurements
|-
!style="background:silver; color:black;" align="left"|Posibilities
|style="background:LightGrey; color:black"|Interferometric profiling||style="background:WhiteSmoke; color:black"|
*Standard microscope imaging
*PSI (Phase Shift Interferometry)
*WLI (White light Interferometry)
*Stitched scans
*Wafer mapping
|-
!style="background:silver; color:black" align="left"|Performance
|style="background:LightGrey; color:black"|With the current 10x objective||style="background:WhiteSmoke; color:black"|
[[:File:Filmetrics Datasheet - Profilm3D Bh6.pdf|See here the data sheet for this instrument]]
|-
|-
!style="background:silver; color:black" align="left"|Substrates
|style="background:LightGrey; color:black"|Substrate size
|style="background:WhiteSmoke; color:black"|
*Substrates no bigger than 100 mm x 100mm
|-
|style="background:silver; color:black"|
| style="background:LightGrey; color:black"|Substrate materials allowed
|style="background:WhiteSmoke; color:black"|
*In principle all materials
|-
|}
 
== Dektak 3ST ==
 
 
[[image:III-V profiler.JPG|300x300px|right|thumb|The profiler placed in 346-904 (Dektak 3ST).]]
 
The Dektak 3ST is intended for profile measurements on samples outside the cleanroom.
 
 
'''The user manual, technical information and contact information can be found in LabManager:'''
 
[http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=184 Dektak 3ST (Dektak) in LabManager]
 
The computer connected to the Dektak 3ST is pretty old and runs Windows 98 SE. It is not connected to the network but traces can be saved on either USB memory stick or floppy disk. The USB driver is an old universal driver and has been shown to work with small size USB sticks. However it did not work with an 8GB Kingston stick.
 
===Equipment performance and process related parameters===
{| border="2" cellspacing="0" cellpadding="10"
|-
!style="background:silver; color:black" align="left" rowspan="4" valign="top" |Performance
|style="background:LightGrey; color:black"|Vertical Range
|style="background:WhiteSmoke; color:black"|
*65 kÅ, 655 kÅ, 1310 kÅ
|-
|style="background:LightGrey; color:black"|Scan length range
|style="background:WhiteSmoke; color:black"|
*50-50000 µm
|-
|style="background:LightGrey; color:black"|Stylus track force
|style="background:WhiteSmoke; color:black"|
*Recommended: 3-10 mg, depending on the softness of the surface
|-
|style="background:LightGrey; color:black"|Scan speed ranges
|style="background:WhiteSmoke; color:black"|
*High speed: 3s for 50µm to 50000µm
*Medium speed: 12s for 50µm to 10000µm
*Low speed: 50s
|-
!style="background:silver; color:black" align="left" rowspan="1" valign="top" |Materials
|style="background:LightGrey; color:black"|Allowed substrate materials
|style="background:WhiteSmoke; color:black"|
*III-V
* Silicon
* polymer
|}
 
 
 
 
 
 
== Stylus Profiler: Dektak150 ==
 
 
[[image:Dektak150.JPG|300x300px|right|thumb|Stylus profiler:Dektak150 placed in 347-183.]]
 
The stylus profiler Dektak150 is intended for profile measurements on samples outside the cleanroom.
 
 
'''The user manual, technical information and contact information can be found in LabManager:'''
 
[http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=457  Stylus profiler:Dektak150 in LabManager]
 
The computer is not connected to the network but data can be saved on a dedicated USB and transfered to a computer on the network.
 
===Equipment performance and process related parameters===
 
{| border="2" cellspacing="0" cellpadding="10"
|-
!style="background:silver; color:black;" align="left"|Purpose
|style="background:LightGrey; color:black"|Profiler for measuring micro structures||style="background:WhiteSmoke; color:black"|
*Single line profiles
*Surface roughness on a line scan
|-
!style="background:silver; color:black" align="left" rowspan="5" valign="top" |Performance
|style="background:LightGrey; color:black"|Scan range x y
|style="background:WhiteSmoke; color:black"|
Line scan x: 50 µm to 55 mm in a single scan
|-
|style="background:LightGrey; color:black"|Scan range z
|style="background:WhiteSmoke; color:black"|
50 Å to 1 mm
|-
|style="background:LightGrey; color:black"|Resolution x y
|style="background:WhiteSmoke; color:black"|
Down to 0.003µm
|-
|style="background:LightGrey; color:black"|Resolution z
|style="background:WhiteSmoke; color:black"|
1Å (@65kÅ), 10Å (@655 kÅ), 80 Å (@5240 kÅ), 160 Å (@1mm)
|-
|style="background:LightGrey; color:black"|Maximum sample thickness
|style="background:WhiteSmoke; color:black"|
100mm
|-
|-
!style="background:silver; color:black" align="left"|Hardware settings
|style="background:LightGrey; color:black"|Tip radius
|style="background:WhiteSmoke; color:black"|
*5 µm 45<sup>o</sup> cone
*0.2 µm 45<sup>o</sup> cone on request
|-
!style="background:silver; color:black" align="left" rowspan="5" valign="top" |Substrates
|style="background:LightGrey; color:black"|Substrate size
|style="background:WhiteSmoke; color:black"|
*Up to 6"
|-
| style="background:LightGrey; color:black"|Substrate materials allowed
|style="background:WhiteSmoke; color:black"|
*In principle all materials
|-
|}