LabAdviser/Courses: Difference between revisions
(202 intermediate revisions by 11 users not shown) | |||
Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@ | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/LabAdviser/Courses click here]''' | ||
'''Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.''' | |||
=Courses= | =Courses= | ||
We are building up a number of courses to educate our users in using the cleanroom facility and the equipment inside. Below you can see the courses that are presently running. The | We are building up a number of courses to educate our users in using the cleanroom facility and the equipment inside along with training for our other facilities. Below you can see the courses that are presently running. The introduction Courses is mandatory for all users that need to use our facilities on their own. Then there is a number of TPT's (Tool Package Training Courses) that you need to attend depending on which kind of tool you need to use inside the facility. | ||
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" | |||
!style="background:Black; color:white" width="3%" align ="center"|Course | |||
!style="background:Black; color:white" width="5%" align ="center"|Mandatory... | |||
!style="background:Black; color:white" width="10%" align ="center"|Short Course Decription | |||
|- | |||
|-style="background:LightGrey; color:black" valign="center" | |||
![https://www.nanolab.dtu.dk/use-nanolab/introduction-course Cleanroom introduction course] | |||
|for working inside the cleanroom | |||
|See the homepage | |||
|- | |||
|- | |||
|-style="background:WhiteSmoke; color:black" valign="center" | |||
![https://www.nanolab.dtu.dk/use-nanolab/other Other Nanolabs facilities introduction course] | |||
|for working in other Nanolab facilities | |||
|See the homepage | |||
|- | |||
|-style="background:LightGrey; color:black" valign="center" | |||
![[/TPT Lithography|TPT Lithography]] | |||
|for working with [[Specific_Process_Knowledge/Lithography|lithography]] | |||
|The course includes theory on lithographic processes and equipment, as well as training in equipment operation and processing in the cleanroom. The course is for all users that intend to perform any kind of lithographic processing in the cleanroom, and is a prerequisite for training in other lithography equipment. | |||
|- | |||
|-style="background:WhiteSmoke; color:black" valign="center" | |||
![[/Mask Design|Mask Design]] | |||
|no | |||
|The course is recommended all users who intend to design their own masks for lithography. | |||
|- | |||
|-style="background:LightGrey; color:black" valign="center" | |||
![[/TPT SEM|TPT SEM]] | |||
|for getting access to SEMs at DTU Nanolab | |||
|The course includes theory about SEM, as well as training in instrument operation. The course is for all users who intend to perform any kind of SEM related process and is a prerequisite for training in any of the SEM in building 314 and 346 at DTU Nanolab and for SEM in building 375. | |||
|- | |||
|-style="background:WhiteSmoke; color:black" valign="center" | |||
![[/TPT Dry Etch|TPT Dry Etch]] | |||
|for getting access to dry etch equipment | |||
|The course includes theory on dry etching and equipment, as well as training in equipment operation in the cleanroom. The course is for all users who intend to perform any kind of dry etching in the cleanroom, and is a prerequisite for training in any of the dry etch equipment. | |||
|- | |||
|-style="background:LightGrey; color:black" valign="center" | |||
![[/TPT Thin Film|TPT Thin Film]] | |||
|for getting access to thin film deposition/growth equipment | |||
|This is a theoretical course introducing the thin film growth and deposition techniques available at DTU Nanolab. The course consists of two lectures. Users that have to use any thin film growth and/or deposition tools in the cleanroom will have to sign up for the lectures, before they apply for a training. | |||
|- | |||
|-style="background:WhiteSmoke; color:black" valign="center" | |||
![https://kurser.dtu.dk/course/10868 Ph.d. course: 10868 Methods in micro and nano fabrication] | |||
|for ph.d. students at Nanolab | |||
|This is a course aimed at PhD students new to work in the DTU Nanolab cleanroom. The objective is to accelerate research projects by providing a fast track learning towards hands-on cleanroom fabrication. To attend the course you MUST have a PhD project (or similar) that require you to work in the DTU Nanolab cleanroom. The course gives you a chance to present and discuss your project with some of your fellow PhD students and experienced process specialists from DTU Nanolab. The TPT courses are a main part of the course. The course gives you 5 ECTS points. | |||
|- | |||
|} | |||
<br clear="all" /> | |||
<!-- | |||
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" | |||
!style="background:Black; color:white" width="5%" align ="center"|Course | |||
!style="background:Black; color:white" width="8%" align ="center"|Intro course | |||
!style="background:Black; color:white" width="10%" align ="center"|TPT Lithography | |||
!style="background:Black; color:white" width="10%" align ="center"|Mask Designing | |||
!style="background:Black; color:white" width="10%" align ="center"|TPT SEM | |||
!style="background:Black; color:white" width="10%" align ="center"|TPT Dry Etch | |||
!style="background:Black; color:white" width="10%" align ="center"|TPT Thin Film | |||
!style="background:Black; color:white" width="10%" align ="center"|Ph.d. course no. 10868 "Methods in micro and nanofabrication" | |||
|- | |||
|-style="background:WhiteSmoke; color:black" valign="top" | |||
!Mandatory ... | |||
|for working inside the cleanroom | |||
|for working with lithography | |||
|no | |||
|for getting access to SEMs at Nanolab building 346 and 314/307 | |||
|for getting access to dry etch equipment | |||
|for getting access to thinfilm deposition/growth equipment | |||
|for ph.d. students at Nanolab | |||
|- | |||
|-style="background:LightGrey; color:black" valign="top" | |||
!Short Course Description | |||
| | |||
|The course includes theory on lithographic processes and equipment, as well as training in equipment operation and processing in the cleanroom. The course is for all users that intend to perform any kind of lithographic processing in the cleanroom, and is a prerequisite for training in other lithography equipment. | |||
|The course is recommended all users who intend to design their own masks for lithography. | |||
| the course includes theory on SEM, as well as training in instrument operation. The course is for all users who intend to perform any kind of SEM related process and is a prerequisite for training in any of the SEM at Nanolab (building 346/314/307). | |||
|the course includes theory on dry etching and equipment, as well as training in equipment operation in the cleanroom. The course is for all users who intend to perform any kind of plasma dry etching in the cleanroom, and is a prerequisite for training in any of the plasma dry etch equipment. | |||
|This is a theoretical course introducing the deposition and growth techniques available at DTU NAnolab. The Users that have to use any thin film growth and/or deposition tools in the cleanroom will have to sign up for the lectures before they apply for a training. | |||
|This is a course aimed at PhD students new to work in the DTU Nanolab cleanroom. The objective is to accelerate research projects by providing a fast track learning towards hands-on cleanroom fabrication. To attend the course you MUST have a PhD project (or similar) that require you to work in the DTU Nanolab cleanroom. | |||
|- | |||
|- | |||
|-style="background:WhiteSmoke; color:black" valign="top" | |||
!Schedule and How to sign up | |||
|See home page | |||
| | |||
'''Theoretical part''' | |||
* Lecture videos that can be viewed at one's leisure. | |||
* A 1 hour "questions and exercises" session 2 times a month (typically Fridays 09:30-10:30). | |||
* '''Sign up via [https://doodle.com/poll/metywuzqziwps6w3 Q&E session Doodle]''' | |||
'''Practical part''' | |||
* A 3-4 hour training session 2 times a month, max. 4 persons per session (typically Wednesdays 09:00 - 12:30 or 10:00 - 13:30). | |||
* '''Sign up via [https://doodle.com/poll/yd2q9tbzm86by2ct Training session Doodle]''' | |||
| | |||
* Self-study using screen cast videoes demonstrating the use of either CleWin og L-edit. | |||
* An exercise where you are guided through the design of a mask. | |||
* All materials are provided on the TPT Mask design page, see link below . | |||
* An optional ½ hour Q&A session with an expert on mask layout. You can make an appointment after finishing the exercise. | |||
| | |||
'''Theoretical part''' | |||
* A 3-hour lecture. The next lectures will be held Monday the 9th of September 2019 from 9:00 to 12:00. Sign up here: [https://danchip.doodle.com/poll/udmcihbbgudyynfy SEM lecture] | |||
'''Practical part''' | |||
* A 2-hour training session, max. 3 persons per session will be planed after the lecture | |||
* A 2-hour one-on-one hands-on session which will request the participant to pass a “driving test” on the SEM. In this session, the participant will have the opportunity to study their own sample | |||
| | |||
'''Theoretical part''' | |||
* 3-hour lecture videos. | |||
* After seeing the videos you must attend a Question&Evaluation session (1-1½ hour), max. 3 persons per session, Please sign up via: [https://doodle.com/poll/awkny9e952arxbxm Dry Etch TPT Lecture doodle]. | |||
*The Question&Evaluation session takes place in room: 347-078 | |||
'''Practical part''' | |||
* 1½ hour video explaining the equipment software. | |||
* A 2 hour training session, max. 3 persons per session will be planed after the Question&Evaluation session. | |||
| | |||
<b>Theoretical part</b> | |||
'''1<sup>st</sup> lecture (2 hours):''' | |||
*An introduction to thin films | |||
*Material properties | |||
*Thermal oxidation | |||
*Electroplating | |||
<i>Sign up here: [https://danchip.doodle.com/poll/k4pdm2n4bpseww5e Thinfilm lecture part1]</i> | |||
'''2<sup>nd</sup> lecture (3 hours):''' | |||
*Vacuum basics | |||
*PVD (physical vapour deposition) | |||
*CVD (chemical vapour depostion) | |||
*ALD (atomic layer deposition) | |||
<i>Sign up here: [https://danchip.doodle.com/poll/4r3ydwzzbrdepgpf Thinfilm lecture part2]</i> | |||
| | |||
*The course gives you a chance to present and discuss your project with some of your fellow PhD students and experienced process specialists from DTU Nanolab. | |||
*The TPT courses are a main part of the course. | |||
*The course gives you 5 ECTS points | |||
|- | |||
|- | |||
|-style="background:LightGray; color:black" valign="top" | |||
!Link to course page - info and preparation material. | |||
|[http://www.nanolab.dtu.dk/english/education/courses/introduction-course Introduction course information on the Nanolab homepage] | |||
|[[/TPT Lithography|TPT Lithography]] | |||
|[[/Mask Design|Mask Design]] | |||
|[[/TPT SEM|TPT SEM]] | |||
|[[/TPT Dry Etch|TPT Dry Etch]] | |||
|[[/TPT Thin Film|TPT Thin Film]] | |||
|[https://kurser.dtu.dk/course/10868 10868 Methods in micro and nano fabrication] | |||
|- | |||
|} | |||
<br clear="all" /> | |||
--> | |||
<!-- | |||
==The Cleanroom Introduction Course== | ==The Cleanroom Introduction Course== | ||
For information regarding the Introduction Course, please take a look at the DTU Danchip homepage, a direct link is given here: [http://www.danchip.dtu.dk/english/education/courses/introduction-course] | For information regarding the Introduction Course, please take a look at the DTU Danchip homepage, a direct link is given here: [http://www.danchip.dtu.dk/english/education/courses/introduction-course] | ||
==The Lithography TPT== | --> | ||
<!-- | |||
==The Lithography TPT == | |||
DTU Danchip offers a Tool Package Training in Lithography; the course includes theory on lithographic processes and equipment, as well as training in equipment operation and processing in the cleanroom. | DTU Danchip offers a Tool Package Training in Lithography; the course includes theory on lithographic processes and equipment, as well as training in equipment operation and processing in the cleanroom. | ||
Line 29: | Line 190: | ||
| | | | ||
<!--'''<span style="color: red;">OBS: The December Litho TPT has been cancelled due to sickness. Contact the Lithography Group for rescheduling if this poses a problem.</span>''' <span style="text-decoration: line-through;">'''NEXT LECTURE: Tuesday 29th of November 9:15 - 13:00 (B347, Seminar room)'''</span>--> | <!--'''<span style="color: red;">OBS: The December Litho TPT has been cancelled due to sickness. Contact the Lithography Group for rescheduling if this poses a problem.</span>''' <span style="text-decoration: line-through;">'''NEXT LECTURE: Tuesday 29th of November 9:15 - 13:00 (B347, Seminar room)'''</span>--> | ||
<!-- | |||
'''Theoretical part''' | '''Theoretical part''' | ||
* Lecture videos that can be viewed at one's leisure. | * Lecture videos that can be viewed at one's leisure. | ||
Line 52: | Line 214: | ||
* Cleanroom safety course at DTU Danchip | * Cleanroom safety course at DTU Danchip | ||
* Admission to the cleanroom must be obtained before the training session | * Admission to the cleanroom must be obtained before the training session | ||
* Theoretical part must be completed before the training session | * Theoretical part must be completed before the training session. | ||
|- | |- | ||
Line 87: | Line 249: | ||
|} | |} | ||
--> | |||
< | <!-- | ||
===Material for preparations and further information=== | ===Material for preparations and further information=== | ||
Line 121: | Line 283: | ||
<br/>On YouTube: | <br/>On YouTube: | ||
*[https://www.youtube.com/watch?v=3JhM3rmLVpA&list=PLjWVU97LayHCX4sz2AH_YiPbNRmkrBYe5 Lithography TPT training videos] | *[https://www.youtube.com/watch?v=3JhM3rmLVpA&list=PLjWVU97LayHCX4sz2AH_YiPbNRmkrBYe5 Lithography TPT training videos] | ||
*[https://www.youtube.com/watch?v=_neUkDsQhsM Training Video: Manual spin coater Labspin] | |||
On DTU Podcasts: | On DTU Podcasts: | ||
*[http://podcast.llab.dtu.dk/fileadmin/podcasts/2016/DTUDanchip/1.055_Spin_Coater_GAMMA_UV-720p.mp4 Training Video: Automatic Spin Coater] | *[http://podcast.llab.dtu.dk/fileadmin/podcasts/2016/DTUDanchip/1.055_Spin_Coater_GAMMA_UV-720p.mp4 Training Video: Automatic Spin Coater] | ||
*[http://podcast.llab.dtu.dk/fileadmin/podcasts/2016/DTUDanchip/1.053_Aligner_MA6_part1_operation-720p.mp4 Training Video: UV Mask Aligner Part I (Operation)] | *[http://podcast.llab.dtu.dk/fileadmin/podcasts/2016/DTUDanchip/1.053_Aligner_MA6_part1_operation-720p.mp4 Training Video: UV Mask Aligner Part I (Operation)] | ||
*[http://podcast.llab.dtu.dk/fileadmin/podcasts/2016/DTUDanchip/1.053_Aligner_MA6_part2_aligning-720p.mp4 Training Video: UV Mask Aligner Part II (Alignment)] | *[http://podcast.llab.dtu.dk/fileadmin/podcasts/2016/DTUDanchip/1.053_Aligner_MA6_part2_aligning-720p.mp4 Training Video: UV Mask Aligner Part II (Alignment)] | ||
*[http://podcast.llab.dtu.dk/fileadmin/podcasts/2016/DTUDanchip/1.050_Developer_TMAH_UV-Lithography-720p.mp4 Training Video: Automatic Puddle Developer] | *[http://podcast.llab.dtu.dk/fileadmin/podcasts/2016/DTUDanchip/1.050_Developer_TMAH_UV-Lithography-720p.mp4 Training Video: Automatic Puddle Developer] | ||
*[http://podcast.llab.dtu.dk/fileadmin/podcasts/2016/DTUDanchip/1.049_Developer_Manual-720p.mp4 Training Video: Manual Puddle Developer] | |||
Line 133: | Line 296: | ||
*Automatic Spin Coater: [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=359 Spin Coater: Gamma UV] | *Automatic Spin Coater: [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=359 Spin Coater: Gamma UV] | ||
<!--*Manual Spin Coater: [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=331 Spin Coater: Manual Standard Resists] --> | <!--*Manual Spin Coater: [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=331 Spin Coater: Manual Standard Resists] --> | ||
<!-- | |||
*UV Mask Aligner: [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=339 Aligner: MA6 - 2] or [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=44 KS Aligner] | *UV Mask Aligner: [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=339 Aligner: MA6 - 2] or [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=44 KS Aligner] | ||
*Automatic Puddle Developer: [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=329 Developer: TMAH UV-lithography] | *Automatic Puddle Developer: [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=329 Developer: TMAH UV-lithography] | ||
<!--*Manual Puddle Developer: [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=324 Developer: TMAH Manual] --> | <!--*Manual Puddle Developer: [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=324 Developer: TMAH Manual] --> | ||
<!-- | |||
'''<big>Process Flows</big>''' | '''<big>Process Flows</big>''' | ||
*[[:Media:Process_Flow_TPT first print.pdf|TPT first print process flow]] | *[[:Media:Process_Flow_TPT first print.pdf|TPT first print process flow]] | ||
Line 145: | Line 309: | ||
|} | |} | ||
--> | |||
<!-- | |||
== The Mask Design TPT == | == The Mask Design TPT == | ||
Line 221: | Line 386: | ||
<br clear="all" /> | <br clear="all" /> | ||
===Material for the Mask Design course=== | ===Material for the Mask Design course=== | ||
{| style="color: black;" width="90%" | {| style="color: black;" width="90%" | ||
Line 227: | Line 394: | ||
| style="width: 20%" valign="top"| | | style="width: 20%" valign="top"| | ||
'''<big>Literature</big>''' | '''<big>Literature</big>''' | ||
* [[media: | * [[media:Beginners guide to mask design using Clewin v1.4.pdf|Beginners guide to Clewin v1.4]] | ||
* [[media:L-Edit User Guide.pdf |L-Edit User Guide]] | * [[media:L-Edit User Guide.pdf |L-Edit User Guide]] | ||
* [[Media:CleWin5UserGuide.pdf| Clewin 5 User Guide]] | * [[Media:CleWin5UserGuide.pdf| Clewin 5 User Guide]] | ||
* [[Specific Process Knowledge | * [[Specific Process Knowledge/Pattern Design#CleWin| How to install CleWin]] | ||
| style="width: 20%" valign="top"| | | style="width: 20%" valign="top"| | ||
Line 249: | Line 416: | ||
<br clear="all" /> | <br clear="all" /> | ||
--> | |||
<!-- | |||
==The Dry Etch TPT == | ==The Dry Etch TPT == | ||
DTU Nanolab offers a Tool Package Training in | DTU Nanolab offers a Tool Package Training in dry etching; the course includes theory on dry etching and equipment, as well as training in equipment operation in the cleanroom. | ||
The course is for all users who intend to perform any kind of plasma dry etching in the cleanroom, and is a prerequisite for training in any of the plasma dry etch equipment's. | The course is for all users who intend to perform any kind of plasma dry etching in the cleanroom, and is a prerequisite for training in any of the plasma dry etch equipment's. | ||
Line 269: | Line 439: | ||
| | | | ||
'''Theoretical part''' | '''Theoretical part''' | ||
* A 3-hour lecture. | * A 3-hour lecture. The lecture is on videos. the videos can be found on YouTube, see link below. You can also find the slides with notes below. It can be helpful to print out the lecture slide for your notes and questions while watching the videos. After seeing the videos you must attend a Question&Evaluation session (1-1½ hour), max. 3 persons per session, Please sign up via: [https://doodle.com/poll/awkny9e952arxbxm Dry Etch TPT Lecture doodle]. The Question&Evaluation session takes place in room: 347-078 | ||
'''Practical part''' | '''Practical part''' | ||
Line 281: | Line 451: | ||
* Room: 347-R078 | * Room: 347-R078 | ||
'''Practical part''' | '''Practical part''' | ||
* The training session takes place inside the cleanroom. The meeting point will be in The gowning area | * The training session takes place inside the cleanroom. The meeting point will be in The gowning area. | ||
|- | |- | ||
Line 287: | Line 457: | ||
!Qualified Prerequisites | !Qualified Prerequisites | ||
| | | | ||
* Cleanroom safety course at DTU | * Cleanroom safety course at DTU Nanolab | ||
* Admission to the cleanroom must be obtained before the training session | * Admission to the cleanroom must be obtained before the training session | ||
|- | |- | ||
Line 295: | Line 465: | ||
| | | | ||
'''Before the Question&Evaluation session''' | '''Before the Question&Evaluation session''' | ||
Watch the lecture videos, see link to the videos below. | *Watch the lecture videos, see link to the videos below. | ||
*If you are not familiar with dry etching we advice you to read through the "Lecture slides with explanatory text included" [[:File:TPT Dry etching April2018 with notes.pdf]] before watching the videos. | |||
'''Before training session''' | '''Before training session''' | ||
* Watch the training video: TPT hands-on intro | * Watch the training video: TPT hands-on intro | ||
* Watch the screen cast video's for the ASE/AOE software | * Watch the screen cast video's for the ASE/AOE software | ||
* Watch the screen cast video's for the DRIE/ICP metal and III-V ICP | * Watch the screen cast video's for the DRIE/ICP metal and III-V ICP<br> | ||
These are on YouTube and you can find a link to the videos below | These are on YouTube and you can find a link to the videos below | ||
|- | |- | ||
Line 307: | Line 478: | ||
!Course Responsible | !Course Responsible | ||
| | | | ||
The Dry Etch Group at DTU Nanolab | '''The Dry Etch Group at DTU Nanolab''' | ||
Jonas Michael-Lindhard | *Jonas Michael-Lindhard | ||
Berit Herstrøm | *Berit Herstrøm | ||
If you have questions you can contact us by e-mailing [mailto:dryetch@danchip.dtu.dk dryetch@danchip.dtu.dk]. | If you have questions you can contact us by e-mailing [mailto:dryetch@danchip.dtu.dk dryetch@danchip.dtu.dk]. | ||
Line 370: | Line 541: | ||
--> | --> | ||
<!-- | |||
| style="width: 20%"| | | style="width: 20%"| | ||
Line 376: | Line 548: | ||
<br clear="all" /> | <br clear="all" /> | ||
--> | |||
<!-- | |||
==The SEM TPT == | ==The SEM TPT == | ||
DTU | DTU Nanolab offers a Tool Package Training in Scanning electron microscope (SEM); the course includes theory on SEM, as well as training in instrument operation. | ||
The course is for all users who intend to perform any kind of SEM related process and is a prerequisite for training in any of the SEM at Danchip. | The course is for all users who intend to perform any kind of SEM related process and is a prerequisite for training in any of the SEM at Danchip. | ||
{|border="1" cellspacing="0" cellpadding="3" align="left" style="text-align:left;" style="width: 70%;" | {|border="1" cellspacing="0" cellpadding="3" align="left" style="text-align:left;" style="width: 70%;" | ||
Line 395: | Line 568: | ||
| | | | ||
'''Theoretical part''' | '''Theoretical part''' | ||
* A 3-hour lecture. The next lectures will be held | * A 3-hour lecture. The next lectures will be held Monday the 9th of September 2019 from 9:00 to 12:00. Sign up here: https://danchip.doodle.com/poll/udmcihbbgudyynfy. | ||
Line 455: | Line 628: | ||
<br clear="all" /> | <br clear="all" /> | ||
=== | ===Slides from the lecture=== | ||
*Lecture slide show [[Media:Danchip_SEM_lecture_January2019_LabAdviser.pptx]] | *Lecture slide show [[Media:Danchip_SEM_lecture_January2019_LabAdviser.pptx]] | ||
<br clear="all" /> | |||
<!-- =[[image:Under_construction.png|200px]]= --> | |||
<!-- | |||
==Thin Film TPT == | |||
DTU Nanolab offers a Tool Package Training (TPT) course in thin film growth and deposition techniques. | |||
Users that have to use any thin film growth and/or deposition tools in the cleanroom will have to sign up for the lectures before they apply for a training. | |||
{|border="1" cellspacing="0" cellpadding="3" align="left" style="text-align:left;" style="width: 70%;" | |||
|- | |||
|- | |||
|-style="background:White; color:black; text-align:center" | |||
!colspan="2"|Thin film tool package training (TPT) | |||
|- | |||
|- | |||
!Schedule | |||
| | |||
<b>Theoretical part</b> | |||
'''1<sup>st</sup> lecture (2 hours):''' | |||
*An introduction to thin films | |||
*Material properties | |||
*Overview of different thin film techniques at DTU Nanolab – 1<sup>st</sup> part: | |||
**Thermal oxidation | |||
**Electroplating | |||
<i>Check the date for when the next lecture will be held and sign up here: https://danchip.doodle.com/poll/k4pdm2n4bpseww5e</i> | |||
<!-- The date will come after the summer vaction--> | |||
<!-- | |||
'''2<sup>nd</sup> lecture (3 hours):''' | |||
*Vacuum basics | |||
*Overview of different thin film techniques at DTU Nanolab – 2<sup>nd</sup> part: | |||
*PVD (physical vapour deposition) | |||
**E-beam evaporation | |||
**Thermal evaporation | |||
**Sputtering | |||
*CVD (chemical vapour depostion) | |||
**LPCVD (low pressure chemical vapour deposition) | |||
**PECVD (plasma enhanced chemical vapour deposition) | |||
*ALD (atomic layer deposition) | |||
<i>Check the date for when the next lecture will be held and sign up here: https://danchip.doodle.com/poll/4r3ydwzzbrdepgpf</i> | |||
<!--The date will come after the summer vaction</i>--> | |||
<!-- | |||
<b>Practical part</b> | |||
* None | |||
|- | |||
|- | |||
!Location | |||
| | |||
'''Theoretical part''' | |||
* The location of the lectures will be notified in the doodles | |||
|- | |||
|- | |||
!Qualified prerequisites | |||
| | |||
* None | |||
|- | |||
|- | |||
!Preparations | |||
| | |||
* None | |||
|- | |||
|- | |||
!Course responsible | |||
| | |||
*The Thin Film group at DTU Nanolab (thinfilm@nanolab.dtu.dk) | |||
|- | |||
|- | |||
!Learning goals | |||
| | |||
*Be aware of relevant material properties for thin films made in the cleanroom | |||
*Understand importance of correct process pressure (for vacuum processes) | |||
*Understand different thin film techniques | |||
*Compare and be able to select appropriate thin film technique | |||
|- | |||
|} | |||
<br clear="all" /> | |||
===Slides from the lectures=== | |||
<big>Slides from lecture 1</big> | |||
*Lecture slide show [[Media:1_DTU_Nanolab_Thin_Film_TPT_final_May2019.pptx]] | |||
<big>Slides from lecture 2</big> | |||
*Lecture slide show [[Media:2_DTU_Nanolab_Thin_Film_TPT_final_May2019.pptx]] | |||
--> | |||
<!-- | |||
== PhD course (10868 Methods in micro and nano fabrication) == | |||
DTU Nanolab offers a PhD course: [https://kurser.dtu.dk/course/10868 | 10868 Methods in micro and nano fabrication] | |||
This is a course aimed at PhD students new to work in the DTU Nanolab cleanroom. The | |||
objective is to accelerate research projects by providing a fast track learning towards hands-on cleanroom fabrication. | |||
To attend the course you MUST have a PhD project (or similar) that require you to work in | |||
the DTU Nanolab cleanroom. | |||
The course gives you a chance to present and discuss your project with some of your fellow PhD students and experienced process specialists from DTU Nanolab. | |||
The TPT courses presented above is a main part of the course. | |||
The course gives you 5 ECTS points | |||
--> | |||
=Links to training videos= | |||
DTU Nanolab has a YouTube channel where we have gathered all our training videos: [https://www.youtube.com/channel/UCJhdUTUJRDNODNiC3V95RQQ] | |||
We have a number of playlists and some single videos for equipment. You can get an overview here with links to the playlists/videos on You Tube | |||
==Safety and behavior== | |||
*Nanolab introduction course: Safety in the Cleanroom [https://www.youtube.com/watch?v=vq5v4xSqH6Q] | |||
*Safety at DTU Nanolab [https://www.youtube.com/watch?v=mKGJfU57vbE] | |||
*Behaviour in the cleanroom at DTU Nanolab [https://www.youtube.com/watch?v=yCVr53mk7rw] | |||
*Playlist: Craftsmen in the cleanroom/håndværkere i renrummet. [https://www.youtube.com/watch?v=D-0T9X9FFBQ&list=PLjWVU97LayHDKnUd0GrKXdqDhRZuI3iwW] | |||
==Labmanager and Labadviser== | |||
*Playlist: DTU Nanolab systems (Labmanager and Labadviser)[https://www.youtube.com/watch?v=jC5soGfyrZc&list=PLjWVU97LayHA_ZKxvmNfTg1Bp53GX07ER] | |||
==Wet chemistry== | |||
*Training in fume hoods part 1 - Intro and Getting Started [https://www.youtube.com/watch?v=DRPHtBAqpU0] | |||
*Training in fume hoods part 2 - Working With Acids, Bases and Solvents [https://www.youtube.com/watch?v=sqqktgLklSs] | |||
*Training in fume hoods part 3 – Wet benches and errors [https://www.youtube.com/watch?v=bvK1ONO1lwM] | |||
*Using Quick Dump Rinse Baths [https://www.youtube.com/watch?v=edMt18Uwq9o&list=PLjWVU97LayHCS7pcUsx1qt7vroSdHciXV] | |||
*Native Silicon Dioxide Removal [https://www.youtube.com/watch?v=4JD-fSWlZac] | |||
==Lithography== | |||
* Playlist: Lithography TPT lecture [https://www.youtube.com/watch?v=hMgpRSOokxE&list=PLjWVU97LayHCHDueZ8qdT1LXJLGr4wLOa] | |||
* Playlist: Litho TPT training videos (equipment) [https://www.youtube.com/watch?v=3JhM3rmLVpA&list=PLjWVU97LayHCX4sz2AH_YiPbNRmkrBYe5] (spin coater, mask aligner, developer) | |||
* E-beam lithography at DTU Nanolab [https://www.youtube.com/watch?v=2bFUO201DS4] | |||
* Playlist: JEOL 9500 EBL Training (New version) [https://www.youtube.com/watch?v=2VVLyVztBEY&list=PLjWVU97LayHAmiPs63f_2Sp-td0vBjTwR] | |||
** JEOL 9500 EBL Training (New version) [https://www.youtube.com/watch?v=2VVLyVztBEY] | |||
** JEOL 9500 EBL Alignment (New version) [https://www.youtube.com/watch?v=kgZ_WNczGzE] | |||
** JEOL 9500 EBL Cassette handling (New version) [https://www.youtube.com/watch?v=vLMgxZQtCL8] | |||
* Playlist: MLA [https://www.youtube.com/watch?v=GyTQNmbev2c&list=PLjWVU97LayHAiCabstMfAUeeWyQoQI_cV] | |||
* Manual spin coater Labspin Training [https://www.youtube.com/watch?v=_neUkDsQhsM] | |||
*Developer: TMAH Manual [https://www.youtube.com/watch?v=btinNzYnLnY&t=2s] | |||
==Thin Film deposition and oxidation== | |||
*Playlist: E-beam evaporator (Temescal) [https://www.youtube.com/watch?v=XNvnv4R8a5o&list=PLjWVU97LayHCQWuQyHwddJnpsEYfQp0wf] | |||
*Lesker dual chamber sputter system at DTU Nanolab [https://www.youtube.com/watch?v=1WHv36coRUc] | |||
*Antistiction treatment [https://www.youtube.com/watch?v=5NrPWXVybXg] | |||
* Furnace training: Oxidation furnace [https://www.youtube.com/watch?v=Hi-1zN1RVqc] | |||
==Dry Etch== | |||
*Playlist: Dry Etch TPT - hands-on videos [https://www.youtube.com/watch?v=ovNM4A4E8Q0&list=PLjWVU97LayHC9cl0cuB65m-FlIScBd5t9] | |||
*Playlist: Dry Etch TPT - Lecture videos [https://www.youtube.com/watch?v=6k6QUyDKQQc&list=PLjWVU97LayHBu0XwMGHss5CdEhka6B72U] | |||
==Characterization== | |||
*Playlist: SEM Training videos for Zeiss Supra SEMs in building 346 [https://www.youtube.com/watch?v=JuFZUsbSHvQ&list=PLjWVU97LayHAIltgr7pUoeIkwiPuP4Qsj] | |||
*Playlist: AFM Icon Nanoscope software training part I/II/III [https://www.youtube.com/watch?v=i6JXopjBiy4&list=PLjWVU97LayHC9xeoG2uv8IaHuY7t-q0Tj] | |||
*Ellipsometer training [https://www.youtube.com/watch?v=EC-oyRhKr0A] | |||
*Playlist: XPS [https://www.youtube.com/playlist?list=PLjWVU97LayHBtOkPCSv8QA-sD4Dbz1jrb] | |||
==Backend tools== | |||
* Disco Dicing saw - blade exchange [https://www.youtube.com/watch?v=0pMraXlfqh8] |
Latest revision as of 09:30, 23 January 2024
Feedback to this page: click here
Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.
Courses
We are building up a number of courses to educate our users in using the cleanroom facility and the equipment inside along with training for our other facilities. Below you can see the courses that are presently running. The introduction Courses is mandatory for all users that need to use our facilities on their own. Then there is a number of TPT's (Tool Package Training Courses) that you need to attend depending on which kind of tool you need to use inside the facility.
Course | Mandatory... | Short Course Decription |
---|---|---|
Cleanroom introduction course | for working inside the cleanroom | See the homepage |
Other Nanolabs facilities introduction course | for working in other Nanolab facilities | See the homepage |
TPT Lithography | for working with lithography | The course includes theory on lithographic processes and equipment, as well as training in equipment operation and processing in the cleanroom. The course is for all users that intend to perform any kind of lithographic processing in the cleanroom, and is a prerequisite for training in other lithography equipment. |
Mask Design | no | The course is recommended all users who intend to design their own masks for lithography. |
TPT SEM | for getting access to SEMs at DTU Nanolab | The course includes theory about SEM, as well as training in instrument operation. The course is for all users who intend to perform any kind of SEM related process and is a prerequisite for training in any of the SEM in building 314 and 346 at DTU Nanolab and for SEM in building 375. |
TPT Dry Etch | for getting access to dry etch equipment | The course includes theory on dry etching and equipment, as well as training in equipment operation in the cleanroom. The course is for all users who intend to perform any kind of dry etching in the cleanroom, and is a prerequisite for training in any of the dry etch equipment. |
TPT Thin Film | for getting access to thin film deposition/growth equipment | This is a theoretical course introducing the thin film growth and deposition techniques available at DTU Nanolab. The course consists of two lectures. Users that have to use any thin film growth and/or deposition tools in the cleanroom will have to sign up for the lectures, before they apply for a training. |
Ph.d. course: 10868 Methods in micro and nano fabrication | for ph.d. students at Nanolab | This is a course aimed at PhD students new to work in the DTU Nanolab cleanroom. The objective is to accelerate research projects by providing a fast track learning towards hands-on cleanroom fabrication. To attend the course you MUST have a PhD project (or similar) that require you to work in the DTU Nanolab cleanroom. The course gives you a chance to present and discuss your project with some of your fellow PhD students and experienced process specialists from DTU Nanolab. The TPT courses are a main part of the course. The course gives you 5 ECTS points. |
Links to training videos
DTU Nanolab has a YouTube channel where we have gathered all our training videos: [1]
We have a number of playlists and some single videos for equipment. You can get an overview here with links to the playlists/videos on You Tube
Safety and behavior
- Nanolab introduction course: Safety in the Cleanroom [2]
- Safety at DTU Nanolab [3]
- Behaviour in the cleanroom at DTU Nanolab [4]
- Playlist: Craftsmen in the cleanroom/håndværkere i renrummet. [5]
Labmanager and Labadviser
- Playlist: DTU Nanolab systems (Labmanager and Labadviser)[6]
Wet chemistry
- Training in fume hoods part 1 - Intro and Getting Started [7]
- Training in fume hoods part 2 - Working With Acids, Bases and Solvents [8]
- Training in fume hoods part 3 – Wet benches and errors [9]
- Using Quick Dump Rinse Baths [10]
- Native Silicon Dioxide Removal [11]
Lithography
- Playlist: Lithography TPT lecture [12]
- Playlist: Litho TPT training videos (equipment) [13] (spin coater, mask aligner, developer)
- E-beam lithography at DTU Nanolab [14]
- Playlist: JEOL 9500 EBL Training (New version) [15]
- Playlist: MLA [19]
- Manual spin coater Labspin Training [20]
- Developer: TMAH Manual [21]
Thin Film deposition and oxidation
- Playlist: E-beam evaporator (Temescal) [22]
- Lesker dual chamber sputter system at DTU Nanolab [23]
- Antistiction treatment [24]
- Furnace training: Oxidation furnace [25]
Dry Etch
Characterization
- Playlist: SEM Training videos for Zeiss Supra SEMs in building 346 [28]
- Playlist: AFM Icon Nanoscope software training part I/II/III [29]
- Ellipsometer training [30]
- Playlist: XPS [31]
Backend tools
- Disco Dicing saw - blade exchange [32]